TECHNET Archives

November 2008

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Fri, 21 Nov 2008 08:11:35 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, [log in to unmask]
Subject:
From:
Werner Engelmaier /* <[log in to unmask]>
Content-Type:
text/plain; charset="utf-8"
In-Reply-To:
Content-Transfer-Encoding:
quoted-printable
MIME-Version:
1.0
Parts/Attachments:
text/plain (1683 lines)
 I know, I know Vladimir,
but alas that is not my definition.
You reduce cavitation/corrosion you need to increase P, to reduce the classical 'Black Pad' you need to reduce P [by either less in the Ni layer and/or reducing number/length of soldering temperature exposure----so quite opposite remedies.
Maybe we need an IPC committee to officially define the situation.

Werner


 


 

-----Original Message-----
From: Igoshev, Vladimir <[log in to unmask]>
To: [log in to unmask]
Sent: Fri, 21 Nov 2008 7:57 am
Subject: Re: [TN] black pad










Hi Werner,

As always, we are going to stick to our preferrences :-)

However, I'd like to highlight that in that ATOTECH paper I sent you a while ago 
stated that the presence of cavitation/corrosion in the layer of E-Ni is the 
major indicator of Black Pad.

Regards,

Vladimir

________________________________

From: [log in to unmask] 
To: Igoshev, Vladimir; [log in to unmask] 
Sent: Thu Nov 20 23:08:06 2008
Subject: Re: [TN] black pad 


Hi Vladimir,
No, I would not agree that the same phenomenological situation should get a 
different name, just because it is caused by a different set of inputs. [The 
solder joint with a fatigue crack is a fatigue failure whether the cause is 
thermo-mechanical loading or purely mechanical loading]. 

'Brittle fracture' as well as 'de-wetting' have already well understood meanings 
different from BP. However, brittle fracture includes BP as well as other 
brittle fractures resulting from other problems.

I=2
0would not call any problems resulting from electroless Ni plating with no or 
insufficient P 'Black Pad'--I have not seen a special name for tis situation.

Having a limited number of pads affected is pretty typical of 'Black Pad'; one 
requirement for BP is the presence of a NiSn-IMC layer. Typical BP does not show 
corrosion/cavitation.

Werner


-----Original Message-----
From: Igoshev, Vladimir <[log in to unmask]>
To: [log in to unmask]; [log in to unmask]
Sent: Thu, 20 Nov 2008 10:31 pm
Subject: Re: [TN] black pad


Good. And since we have agreed that different thenomenon (root causes) can cause 
almost identical appearance (Black), then would it be logical to use a different 
name for each of them (Black Pad; Brittle Fracture: Dewetting, etc.) .

Just to give an example, a few days ago I came accross two different problems 
with ENIG and I still don't know what had caused them (to be exact, I suspect 
the root cause in both cases is in the plating process).

The reason I mentioned about them is that both could have been easily (and 
wrongly) called Black Pad, as the pads were dark (as usual after joint is broken 
or not formed. However, in one case only limited numer of pads exhibited the 
problem, and the layer of E-Ni was not corroded/cavitated (ruling out Black Pad, 
as I understand it). In the second case, E-Ni had NO phosphorus in it (at least 
I couldn't detect it with EDS) and I know it was supposed to be Ni-P, not Ni-B.
U don't even know how to call that=2
0case, but definitely not Black Pad :-)

Regards,

Vladimir


----- Original Message -----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Thu Nov 20 18:17:42 2008
Subject: Re: [TN] black pad


 Agreed, the prescription for the fix will be different.

Werner







-----Original Message-----
From: Igoshev, Vladimir <[log in to unmask]>
To: [log in to unmask]
Sent: Thu, 20 Nov 2008 5:52 pm
Subject:20Re: [TN] black pad










Hi Werner,

I completely agree on what we disagree on :-)

I think that the same appearnce can (and is in that particuar case) be caused by
completely different phenomena, therefore the recepie to fix/avoid it will be
different.

Regards,

Vladimir

----- Original Message -----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Thu Nov 20 17:28:06 2008
Subject: Re: [TN] black pad


 Hi Vladimir,
That is where we disagree--the definition of 'Black Pad.'
I define it as the phenomenon root cause regardless of what caused it--that is
not to say that who caused it is unimportant.

Werner







-----Original Message-----
From: Igoshev, Vladimir <[log in to unmask]>
To: [log in to unmask]
Sent: Thu, 20 Nov 2008 5:20 pm
Subject: RE: [TN] black pad





























Hi Werner,



 

0A

I should have referred to your exact phrase,
so you wouldn’t have to correct me J



As far as the definition of BP is
concerned, then I still prefer to define it 
as a manufacturing defect, which
has nothing to do with the assembly process.



The presence of thicker P-enriched layer
isn’t a good thing but in true cases of BP it’s normal
(thickn
ess-wise) but the joints has almost zero strength.





Regards,



 



Vladimir



 
















From:
[log in to unmask] [mailto:[log in to unmask]]

Sent: Thursday, November 20, 2008
5:06 PM

To: [log in to unmask]; Igoshev,
Vladimir

Subject: Re: [TN] black pad






 






Hi Vladimir,

I did not say 'excessive temperature'-- I said 'the more you expose
an ENIG layer to soldering temperatures'--that means multiple or lengthy
exposures.

If you define 'Black Pad' as the presence of P at the Ni/NiSn-IMC interlayer to
a degree significantly weakening that i nterface, then you can arrive at that
condition by
 multiple paths.

One is faulty manufacturing, the other is excessive Ni-dissolution--of course,
these can work in combination.



Werner









 









 






-----Original
Message-----

From: Igoshev, Vladimir <[log in to unmask]>

To: [log in to unmask]

Sent: Thu, 20 Nov 2008 4:45 pm

Subject: Re: [TN] black pad




Well, with all due respect I would have to disagree with you Werner (not





for the first time :-)). I wouldn't associate Black Pad with excessive





soldering temperature. It's rather a board manufacturing related issue.











Regards,












Vladimir











-----Original Message-----





From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier /*





Sent: Thursday, November 20, 2008 4:38 PM

0A


To: [log in to unmask]





Subject: Re: [TN] black pad

















 The more you expose an ENIG layer to soldering temperatures, the more





Ni dissolves leaving more P at the layer between the Ni and the





NiSn-IMC. The more? P the weaker this interface, leading to 'Black Pad'











Werner

















 

















 











-----Original Message-----





From: henry rekers <[log in to unmask]>





To: [log in to unmask]





Sent: Thu, 20 Nov 2008 3:41 pm





Subject: Re: [TN] black pad


=0
A


0A


























































Can you give me any examples of black pad being caused by anything other





than a





"bad board"? ie.? Is there anything in processing "perfect board" that





would





cause a de-wet condition that indicates black pad??? I guess where I'm





going is,





can this be anything other than a supplier issue?











--- On Thu, 11/20/08, Werner Engelmaier /* <[log in to unmask]> wrote:











From: Werner Engelmaier /* <[log in to unmask]>



=0
A
Subject: Re: [TN] black pad





To: [log in to unmask]


0A


Received: Thursday, November 20, 2008, 1:26 PM











 Hi 'rekers,'





You canno
t broad-brush like this. Some FAB houses do quite well, others





not.





ENIG, from various sources and at various conditions, has shown nickel





corrosion or high phosphide concentrations. The underlying reasons for





these are





different, actually diametrically opposed. Some are the fault of the FAB





house





others not.











Werner

















 

















 











-----Original Message-----





From: henry rekers <[log in to unmask]>





To: [log in to unmask]




Sent: Thu, 20 Nov 2008 12:45 pm


=0
A

Subject: [TN] black pad

































































Anybody out there experiencing mass dewetting issues from North American





board





shops?





?





From what I understand primary causes for dewetting (assuming the





reflow/wave





profile is bang on) is all on the board, ie nickel corrosion,





degeneration of





the nickel, or outgassing of the nickel/copper.? (I'm talking enig





here.)





?





Anybody?

















      ___
_______________________________________________________________





Connect with friends from any web browser - no download required. Try





the new






Yahoo! Canada Messenger for the Web BETA at





http://ca.messenger.yahoo.com/webmessengerpromo.php











---------------------------------------------------





Technet Mail List provided as a service by IPC using LISTSERV 15.0





To unsubscribe, send a message to [log in to unmask] with following text





in





the BODY (NOT the subject field): SIGNOFF Technet





To temporarily halt or (re-start) delivery of Technet send e-mail to





[log in to unmask]: SET Technet NOMAIL or (MAIL)





To receive ONE mailing per day of all the posts: send e-mail to





[log in to unmask]: SET Technet Digest





Search
 the archives of previous posts at:





http://listserv.ipc.org/archives





Please visit IPC web site





http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for





additional information, or contact Keach Sasamori at [log in to unmask] or





847-615-7100 ext.2815





-----------------------------------------------------























 

















---------------------------------------------------





Technet Mail List provided as a service by IPC using LISTSERV 15.0





To unsubscribe, send a message to [log in to unmask] with following text





in





the BODY (NOT the subject field): SIGNOFF Techn
et





To temporarily halt or (re-start) delivery of Technet send e-mail to
=0 A 




[log in to unmask]: SET Technet NOMAIL or (MAIL)


=0
A

To receive ONE mailing per day of all the posts: send e-mail to





[log in to unmask]: SET Technet Digest





Search the archives of previous posts at:





http://listserv.ipc.org/archives





Please visit IPC web site





http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for





additional information, or contact Keach Sasamori at [log in to unmask] or





847-615-7100 ext.2815





-----------------------------------------------------























      __________________________________________________________________





Instant Messaging, free SMS, sharing photos and more... Try the new





Yahoo!






Canada Messenger at http://ca.beta.messenger.yahoo.com/











---------------------------------------------------





Technet Mail List provided as a service by IPC using LISTSERV 15.0





To unsubscribe, send a message to [log in to unmask] with following text





in





the BODY (NOT the subject field): SIGNOFF Technet





To temporarily halt or (re-start) delivery of Technet send e-mail to





[log in to unmask]: SET Technet NOMAIL or (MAIL)





To receive ONE mailing per day of all the posts: send e-mail to





[log in to unmask]: SET Technet Digest





Search the archives of previous posts at:





http://listserv.ipc.o
rg/archives





Please visit IPC web site





http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for





addition al information,
or contact Keach Sasamori at [log in to unmask] or





847-615-7100 ext.2815





-----------------------------------------------------























 

















---------------------------------------------------





Technet Mail List provided as a service by IPC using LISTSERV 15.0





To unsubscribe, send a message to [log in to unmask] with following text





in





the BODY (NOT the subject field): SIGNOFF Technet





To temporarily halt or (re-start) delivery of Technet send e-mail to





[log in to unmask]: SET Technet NOMAIL or (MAIL)





To receive ONE mailing per day of all20the posts: send e-mail to





[log in to unmask]: SET Technet Digest





Search the archives of previous posts at:





http://listserv.ipc.org/archives





Please visit IPC web site





http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional





information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100





ext.2815





-----------------------------------------------------











---------------------------------------------------





Technet Mail List provided as a service by IPC using LISTSERV 15.0





To unsubscribe, send a message to [log in to unmask] with following text in





the BODY (NOT the subject field): SIGNOFF Technet

=0
A


To temporarily halt or (re-start) delivery of Technet send e-mail to





[log in to unmask]: SET Technet NOMAIL or (MAIL)
0A



To receive ONE mailing per day of all the posts: send e-mail to





[log in to unmask]: SET Technet D igest





Search the archives of previous posts at: http://listserv.ipc.org/archives





Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for





additional information, or contact Keach Sasamori at [log in to unmask] or





847-615-7100 ext.2815





-----------------------------------------------------













 













Traveling
over the river or through the woods this holiday season? Get
the MapQuest Toolbar. Directions, Traffic, Gas Prices & More!












---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receiv e ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------







-----
----------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for 
additional information, or contact Keach Sasamori at [log in to unmask] 
<mailto:sasak [log in to unmask]>  or 847-615-7100 ext.2815
-----------------------------------------------------



________________________________

Traveling over the river or through the woods this holiday season? Get the 
MapQuest Toolbar <http://pr.atwola.com/promoclk/100000075x1212816426x1200798402/aol?redir=http://www.mapquest.com/toolbar?ncid=emlwemqmq00000001> 
. Directions, Traffic, Gas Prices & More! 



 


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2