TECHNET Archives

June 2011

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
"Stadem, Richard D." <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Stadem, Richard D.
Date:
Thu, 2 Jun 2011 11:16:13 -0500
Content-Type:
text/plain
Parts/Attachments:
text/plain (241 lines)
To address one of the goal's of the selected finish, as well as Hillman's skill at selecting a good time to go on vacation; be sure to get even.

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Douglas Pauls
Sent: Thursday, June 02, 2011 11:00 AM
To: [log in to unmask]
Subject: Re: [TN] Best Board Finish - beyond gold

That's because Dave is on vacation kayaking in North Carolina and I am 
buried beyond belief.

Doug Pauls



"Wenger, George M." <[log in to unmask]> 
Sent by: TechNet <[log in to unmask]>
06/02/2011 10:56 AM
Please respond to
TechNet E-Mail Forum <[log in to unmask]>; Please respond to
"Wenger, George M." <[log in to unmask]>


To
<[log in to unmask]>
cc

Subject
Re: [TN] Best Board Finish - beyond gold






Barbara,

I've never met Richard but I've always agreed with his comments on TN. The 
only thing I can add which I absolutely believe is that you need to do two 
things; 1st is to listen to users of surface finishes like Richard and 
Joyce) not suppliers of surface finished PCBs or suppliers of surface 
finish chemistries because the users will tell you what works for them and 
the suppliers will tell you what they need to for you to buy their 
products and 2nd you should run trials before you switching.

HASL (i.e., SnPb HASL not Pb-Free HASL) is a great choice if you don't 
need to be RoHS 6/6 compliant and you don't have fine pitch assembly
OSP and ImAg are good choices for fine pitch assembly.
From my participation many years ago on NCMS PCB Surface Finish program I 
have bias against Pd surface finishes.
From my participation many years ago on NCMS Pb-Free program I have bias 
against ImSn.
I'm a little surprised that no one has come forth to recommend switching 
to ImSn or to stay with ENIG.
I'm also a little surprised you haven't gotten Doug's "it depends" comment 
yet.
I'm also a little surprised you haven't gotten Dave's comment about using 
all surface finishes and they work.

I do think that Richard, Frank and I have a bias toward ImAg because it 
works well for our products and I think if you spoke to others who use 
multiple surface finishes they will also indicate ImAg works well.

Regards,
George
George M. Wenger
Senior Principal Reliability / FMA Engineer
Andrew Corporation - Wireless Network Solutions
40 Technology Drive, Warren, NJ 07059
(908) 546-4531 Office (732) 309-8964 Mobile
E-mail: [log in to unmask]

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stadem, Richard D.
Sent: Thursday, June 02, 2011 10:46 AM
To: [log in to unmask]
Subject: Re: [TN] Best Board Finish - beyond gold

I agree with everything you say, Barbara. It sounds like you are now on 
your way to making the correct choice.
Stay away from immersion tin.
If you choose immersion silver, refer to both IPC 1601 and IPC 4553 for 
storage and handling considerations. They can be managed.
The double-sided process can leave a slight reduction of solderability 
with immersion silver PWBs by the time you are ready to hand solder any 
PTH parts, making that more difficult to do, sometimes.
That is why I asked.
Also, if you select Immersion Silver,  make sure that your PWB fabricator 
has a good plating product, a well controlled process and some experience 
with it.
Ditto with ENIG. Especially with ENIG.
Regarding immersion silver, it is susceptible to environments that are 
heavy in sulfides, such as automotive exhaust, rubber processing, or paper 
processing. Keep some of these things in mind both from an end-use 
environment standpoint and from a storage standpoint. Do not store in 
areas where there are open containers of soaps, fluxes, etc., nearby.

From: Barbara Burcham [mailto:[log in to unmask]]
Sent: Thursday, June 02, 2011 9:22 AM
To: Stadem, Richard D.
Cc: TechNet E-Mail Forum
Subject: Re: [TN] Best Board Finish - beyond gold

Thanks everyone for you imput. What a great group of people!

Richard,
The application will be double sided, fine pitch array components, some 
through hole components and going into a shock environment.
I will need to connect with the assemblers to check on flux and paste 
compounds. Does this information help?  You make an excellent point. Must 
have the total picture. I do not know, yet, how long boards will sit on 
the shelf before moving into assembly, either. I do know that shelf life 
will also impact this decision.
I do not think that I want to use tin...that hairy growth stuff.
Barbara



On Thu, Jun 2, 2011 at 8:01 AM, Stadem, Richard D. <[log in to unmask]<
mailto:[log in to unmask]>> wrote:
Barbara,
What is the application, board type, component types, etc?
Immersion silver is my personal favorite, but that is completely 
irrelevant.
You should choose a board finish dependent upon the application of the 
CCA, whether it has fine-pitch array components, including CSPs, whether 
it is double-sided with PTH parts or hand-soldered components, the 
environment the CCA will be used in, the flux type to be used, the alloy 
that is required, and several other factors that go into the decision. 
Without complete knowledge of all these factors, it is hard for anyone to 
answer that question. I can tell you that IAg beats ENIG in cost, but each 
finish has strengths and weaknesses. Some definitely have more or less 
than others.



-----Original Message-----
From: TechNet [mailto:[log in to unmask]<mailto:[log in to unmask]>] On Behalf 
Of Barbara Burcham
Sent: Wednesday, June 01, 2011 8:17 PM
To: [log in to unmask]<mailto:[log in to unmask]>
Subject: [TN] Best Board Finish - beyond gold
Hey Y'all,
I am looking for a reliable bare board finish that beats the cost of gold.
What experience is out there?
What would you recommend?
Thanks,
Barbara Burcham
pcb Trace Design
[log in to unmask]<mailto:[log in to unmask]>

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]<
mailto:[log in to unmask]>
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask]<mailto:[log in to unmask]
> with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]<mailto:[log in to unmask]>: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]<mailto:[log in to unmask]>: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask]<
mailto:[log in to unmask]> or 847-615-7100 
ext.2815<tel:847-615-7100%20ext.2815>
-----------------------------------------------------


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------



______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2