Hi Technet,
Yesterday I visited one of our bare board manufacturers and had a close
look at their HASL-process. The reason for the visit was solderability
problems on BGA-pads, which sometimes look thin and dull. Occasionally
copper seems to be visible through the tinlead.
In general I think this is a very professional boardshop, but (being
not an expert) I don't know what to think about their HASL-process. I
hope someone on this great forum is willing to give me some input on my
findings, in terms of good or bad, or possibilities for improvement:
Machine: Quicksilver SM, vertical HASL, 250 kg solderpot, no preheat
Time between microetch (drying) and fluxing can be up to two hours
Solder pot temperature set to 255 °C
Leveling is done is such a way that the solder is as flat as possible,
although the design of the airknives causes a big difference betweeen
the two boardsides. With XRF we measured a thickness of only 0.4 microns
on BGA-pads, with about 3 microns on similar pads on the other
boardside.
Water-based flux from an open tank, without any composition control,
but tank is replaced every 24 hours.
Solder is replaced every 6 months, but except for copper contamination
no composition-check is ever done.
When copper is above 0.3 % the dross is skimmed off to assure that
copper content stays below 0.35 %.
Throughput of the machine is about 700 panels per day.
Daan Terstegge
Thales Communications
Unclassified mail
Personal Website: http://www.smtinfo.net
---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|