Werner
Tg is not a fixed value, even for a single given sheet of laminate. It
can drop by 30°C or possibly more depending on the history of the resin,
for example, if it has been subjected to a humid atmosphere or to the
vapours of certain chemicals. If you extend it to multiple sheets, those
sheets nearest the platens in the laminating press will have a different
Tg to those in the centre of the pile, because the temp profile is not
the same. Then, when it's a matter of different batches of resin mix...,
treater drying cycle..., prepreg age before pressing... etc., the
tolerance becomes very significant, even at the laminator's goods-out
door. By the time it reaches the assembler, a ± 25-30°C tolerance could
be normal.
This does not take into account the tolerance of measurement of a
physical phenomenon which is gradual in its application (the Tg depends
on the polymer MW, which is quite variable); there is no sharply defined
transition from a conchoidal fracture to a fluage.
Brian
Werner Engelmaier wrote:
> Hi Doug,
> Of course I do not suggest Tg 178 instead of 175; but the slash sheets give
> ranges on the same sheet thast include Tg's with 50 degree differences--they
> should perhaps be no ore than about 20.
>
>
>
> Werner
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
> -----------------------------------------------------
>
--
http://www.cypenv.org Cyprus environment/energy
http://www.cypenv.org/worldenv World environment/energy
http://www.cypenv.org/weather Cyprus weather
http://www.cypenv.org/smf/index.php Environment/energy forums
http://groups.yahoo.com/group/cypnature/ Cyprus nature forum
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|