TECHNET Archives

January 2008

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Lee parker <[log in to unmask]>
Date:
Tue, 29 Jan 2008 05:28:35 +0200
MIME-version:
1.0
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Gabriela Bogdan <[log in to unmask]>
Content-type:
text/plain; format=flowed; charset=iso-8859-1; reply-type=response
Subject:
From:
Gabriela Bogdan <[log in to unmask]>
Content-transfer-encoding:
7BIT
Parts/Attachments:
text/plain (210 lines)
Yes, I know, it is our preferred coating also, just had by bad luck  two 
batches from two different suppliers with excessive microvoids, that's what 
made me start the discussion.
Thank you all,
Gaby
----- Original Message ----- 
From: "Lee parker" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Monday, January 28, 2008 10:14 PM
Subject: Re: [TN] Microvoids immersion silver


> Gaby
>
> There is no reason to suspect that soldering issues of any kind will be 
> aggravated by immersion silver provided the chemistry is up to par, the 
> process is within the bath supplier's spec and there is an adequate 
> quality control process in place. Immersion silver has been widely used by 
> many OEMs with great success, AT&T, Andrew etc. Immersion sliver voids 
> have been reported by some suppliers, but most of these issues were 
> resolved by the MacDermid  study, I imagine Danny Fritz can get you a copy 
> of the paper. I installed this process in the AT&T Richmond Works in 95. I 
> have not heard of any soldering issues that were not quickly resolved, 
> certainly nothing on the order of black pad.
>
> I would certainly qualify any potential supplier to verify the process 
> meets the vendor's spec and that a quality control plan is in place and on 
> going. I would also monitor the quality of the silver coating (thickness 
> measurements, cross sections and solderability assessments etc.) If the 
> quality of the coating is robust over a extended period of time, I would 
> then begin to expand the inspection interval.
>
> To insure a quality product from all stand points it is absolutely 
> necessary to continuously monitor the supplier with on site visits whether 
> the supplier is on shore or off shore. This of course is one of the 
> disadvantages of off shore suppliers.
>
> Best regards
>
> Lee
>
> J. Lee Parker, Ph.D.
> JLP Consultants LLC
> 804 779 3389
>
>
> ----- Original Message ----- 
> From: "Gabriela Bogdan" <[log in to unmask]>
> To: <[log in to unmask]>
> Sent: Monday, January 28, 2008 1:30 PM
> Subject: Re: [TN] Microvoids immersion silver
>
>
>> Thank you all for your information.
>> Now, next:
>> Opens in BGA on Immersion silver.
>> MICROvoids detected by X-ray on : free pads, ordinary smt joints, BGA 
>> solder
>> joints (ball to circuit pad location).
>> BGA rework?
>> BGA replacement?
>> SCRAP??????
>> I fear that the story begins to be similar to the black pad nightmare 
>> with
>> immersion gold.....
>> Gaby
>> ----- Original Message ----- 
>> From: "Dennis Fritz" <[log in to unmask]>
>> To: <[log in to unmask]>
>> Sent: Monday, January 28, 2008 8:17 PM
>> Subject: Re: [TN] Microvoids immersion silver
>>
>>
>> >I will try to answer each question as you ask them.
>> >
>> > In a message dated 1/28/2008 12:32:15 P.M. Eastern Standard Time,
>> > [log in to unmask] writes:
>> >
>> > Dear  Netters,
>> > Is there a preferred process for immersion silver finish in order  to
>> > minimize microvoids?
>> > Immersion silver vendors have a preferred way for fabricators to 
>> > operate
>> > the
>> > immersion silver line to minimize/prevent microvoids.  Please 
>> > understand
>> > there are more effects than just the immersion silver bath itself.
>> >
>> >
>> > How  do you choose the preferred immersion silver PCB supplier?
>> > Your board supplier is very interactive in the performance of immersion
>> > silver boards.  The best plating solution, run poorly by a fabricator 
>> > can
>> > give
>> > problems and vice versa.  Obtain boards from more than one fabricator 
>> > and
>> > from
>> > various bath suppliers.  Probably, the bath vendor has an opinion, 
>> > from
>> > process audits, how each fabricator is obeying the process information 
>> > in
>> > the data
>> > sheets.  See what works best with your solder paste and wave  solder.
>> > Wetting balance, dip-and-look, solder spread are all tests that 
>> > indicate
>> > good
>> > performance.
>> >
>> >
>> > Which test for bare boards could give the best  information?
>> > IPC J-standard 003 for board solderability should be a guide for your
>> > operation.  Do you use international IEC standards?
>> >
>> >
>> > Should I perform a print and reflow test for each batch, followed  by
>> > x-ray?
>> > The print/reflow test is a good idea, with controlled conditions. 
>> > However,
>> > I
>> > don't think you will see microvoids with X-ray.  You probably need 
>> > cross
>> > sectioning to see microvoids.
>> >
>> >
>> > Which tests are the suppliers performing?
>> > By suppliers, do you mean board fabricators or plating chemistry
>> > suppliers?
>> > This is not a one stop shop. The board shop should be  running process
>> > controls on their microetch for roughness and silver  immersion plating
>> > bath.  The
>> > plating rate and final thickness are  recommended by the bath supplier,
>> > and
>> > should be obeyed in fabrication. Both shop  and supplier may be running
>> > assembly
>> > simulation and then cross sectioning to see  if there are any 
>> > microvoids.
>> >
>> >
>> > Thanks,
>> > Gaby
>> >
>> > Dennis Fritz
>> > MacDermid, Inc.
>> >
>> >
>> >
>> > **************Start the year off right.  Easy ways to stay in shape.
>> > http://body.aol.com/fitness/winter-exercise?NCID=aolcmp00300000002489
>> >
>> > ---------------------------------------------------
>> > Technet Mail List provided as a service by IPC using LISTSERV 15.0
>> > To unsubscribe, send a message to [log in to unmask] with following text 
>> > in
>> > the BODY (NOT the subject field): SIGNOFF Technet
>> > To temporarily halt or (re-start) delivery of Technet send e-mail to
>> > [log in to unmask]: SET Technet NOMAIL or (MAIL)
>> > To receive ONE mailing per day of all the posts: send e-mail to
>> > [log in to unmask]: SET Technet Digest
>> > Search the archives of previous posts at: 
>> > http://listserv.ipc.org/archives
>> > Please visit IPC web site 
>> > http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>> > for additional information, or contact Keach Sasamori at [log in to unmask] 
>> > or
>> > 847-615-7100 ext.2815
>> > -----------------------------------------------------
>> >
>>
>> ---------------------------------------------------
>> Technet Mail List provided as a service by IPC using LISTSERV 15.0
>> To unsubscribe, send a message to [log in to unmask] with following text in
>> the BODY (NOT the subject field): SIGNOFF Technet
>> To temporarily halt or (re-start) delivery of Technet send e-mail to 
>> [log in to unmask]: SET Technet NOMAIL or (MAIL)
>> To receive ONE mailing per day of all the posts: send e-mail to 
>> [log in to unmask]: SET Technet Digest
>> Search the archives of previous posts at: 
>> http://listserv.ipc.org/archives
>> Please visit IPC web site 
>> http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional 
>> information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 
>> ext.2815
>> -----------------------------------------------------
>>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to 
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to 
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 
> for additional information, or contact Keach Sasamori at [log in to unmask] or 
> 847-615-7100 ext.2815
> -----------------------------------------------------
> 

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2