Pressfit works fine with a variety of surface finishes. Do it with
ENIG. Do it with OSP. Do it with Solder Coated. Do it with Immersion
Silver. Just make sure you do the important stuff right.
That is:
* Drill size: use the precise drill size specified by connector Mfg
* Cu thickness: have at least the minimum specified annular copper
* Min hole size: don't let the hole get too small (overplated) or
you're choke your press or "Z-in" your pins to the board surface
* Verify if you're serious about it: retention force and hole
wall deformation and min remaining hole wall copper (the old
Bellcore std is really the benchmark for this testing)
At 03:47 PM 10/22/2010, Robert Kondner wrote:
>Interesting. My concept of press fit was the swaging of soft solder material
>helped form a gas tight connection.
>
> I am curious to here how this thread comes out.
>
>Bob K.
>
>
>
>-----Original Message-----
>From: TechNet [mailto:[log in to unmask]] On Behalf Of Victor Hernandez
>Sent: Friday, October 22, 2010 9:46 AM
>To: [log in to unmask]
>Subject: [TN] Press Pin Fits connector
>
>Fellow TechNetters:
>
> What are the Pros & Cons of using PPF connector with a board surface
>finish of ENIG? I typically see PPF connector on other than ENIG plating.
>
>Victor, " X "
>
>
>______________________________________________________________________
>This email has been scanned by the MessageLabs Email Security System.
>For more information please contact helpdesk at x2960 or [log in to unmask]
>______________________________________________________________________
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------
>
>
>______________________________________________________________________
>This email has been scanned by the MessageLabs Email Security System.
>For more information please contact helpdesk at x2960 or [log in to unmask]
>______________________________________________________________________
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site
>http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
>information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|