TECHNET Archives

August 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Mime-Version:
1.0
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, John Burke <[log in to unmask]>
Date:
Wed, 17 Aug 2005 14:31:45 -0600
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Steve Hodge <[log in to unmask]>
Subject:
From:
Steve Hodge <[log in to unmask]>
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"; format=flowed
Parts/Attachments:
text/plain (115 lines)
I believe the process for the selective solder over nickle (RLM) used
tin/nickel and not pure sulfamate nickel. In the case I cited, we had to
put on the immersion gold to prevent passivation in between nickel and HASL
processes.

At 02:12 PM 08/17/2005, you wrote:
>Which works for a plating process, not too sure if the same applies where
>the nickel is happily oxidising all of the time it is out of a plating tank.
>
>John
>
>------------------------------------
>Avanex
>John Burke
>Senior Manager RoHS Compliance
>[log in to unmask]
>40919 Encyclopedia Circle
>Fremont
>CA 94538
>tel: 510 897 4250
>fax: 510 979 0189
>mobile: 510 676 6312
>------------------------------------
>
>
>-----Original Message-----
>From: TechNet [mailto:[log in to unmask]]On Behalf Of Scott B. Westheimer
>Sent: Wednesday, August 17, 2005 1:01 PM
>To: [log in to unmask]
>Subject: Re: [TN] HASL over nickel
>
>
>The was actually a process back in the 70's called RLM. For you that worked
>in Silicon Valley back then it stood for Robert L Mac the owner of Santa
>Clara Circuits who had the process patented. It was a nickel plated board
>that was then covered completed with screen ink, sorry no dry film back
>then, except for the pads and then tin leaded plated and reflowed. Was there
>any issues? Not sure but there was a lot of boards made that way, for
>several years.
>
>Scott B. Westheimer
>Colonial Circuits
>----- Original Message -----
>From: "Tom Moore" <[log in to unmask]>
>To: <[log in to unmask]>
>Sent: Wednesday, August 17, 2005 3:38 PM
>Subject: [TN] HASL over nickel
>
>
> > Our PC board supplier inadvertently supplied us with boards composed of
> > gold over nickel rather than the specified HASL finish. While we kept some
> > of the boards to keep our production line running, we sent the rest back
> > to
> > have the gold stripped off and run through the HASl process. Now our
> > supplier is telling us that they will not be able to remove the nickel
> > that
> > has bonded to the copper pads. I'm going to have the supplier guarantee
> > the
> > board life in blood, but I would feel more confident in having
> > confirmation
> > by this group's expertise. Thanks for your help.
> >
> > ---------------------------------------------------
> > Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> > To unsubscribe, send a message to [log in to unmask] with following text in
> > the BODY (NOT the subject field): SIGNOFF Technet
> > To temporarily halt or (re-start) delivery of Technet send e-mail to
> > [log in to unmask]: SET Technet NOMAIL or (MAIL)
> > To receive ONE mailing per day of all the posts: send e-mail to
> > [log in to unmask]: SET Technet Digest
> > Search the archives of previous posts at: http://listserv.ipc.org/archives
> > Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> > for additional information, or contact Keach Sasamori at [log in to unmask] or
> > 847-615-7100 ext.2815
> > -----------------------------------------------------
> >
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 1.8e
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 1.8e
>To unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet
>To temporarily halt or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL)
>To receive ONE mailing per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at: http://listserv.ipc.org/archives
>Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask] or
>847-615-7100 ext.2815
>-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2