Gold reacts with copper, thus the nickel barrier. I have many examples
of nickel skips, the copper migrates up through the gold and you get a
bright orange colored pad that you cannot solder to.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Phillip Bavaro
Sent: Monday, January 07, 2008 3:03 PM
To: [log in to unmask]
Subject: Re: [TN] OSP w selective gold
Is it true that eliminating the nickel step affects the wetting
properties, and therefore selective gold is only used as a
non-solderable conductive contact surface?
At 07:06 PM 1/4/2008 -0500, Lee parker wrote:
>Genny
>
>OSP/immersion gold (I assume you are alluding to immersion gold) boards
>have been fabricated in Asia for several years for the cellular phone
>handset industry. The big issue I am aware of is in fabrication of the
>board; it has been necessary to use particular immersion gold
>processes, which your fab has is probably aware of.
>
>Best regards
>
>Lee
>
>J. Lee Parker, Ph.D.
>JLP Consultants LLC
>804 779 3389
>
>
>----- Original Message -----
>From: "Genny Gibbard" <[log in to unmask]>
>To: <[log in to unmask]>
>Sent: Thursday, January 03, 2008 5:22 PM
>Subject: [TN] OSP w selective gold
>
>
>We have never used OSP for anything, but we may be required to switch
>one of our products to it. Can anyone point me in the direction of
>some good solid info regarding working with this finish?
>How common is it, especially if you need selective gold? Are there any
>solder process pitfalls to watch out for?
>This is for leadfree products.
>
>Thanks in advance,
>Genny.
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
>unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
>or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
>per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at:
>http://listserv.ipc.org/archives Please visit IPC web site
>http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask]
>or 847-615-7100 ext.2815
>-----------------------------------------------------
>
>---------------------------------------------------
>Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
>unsubscribe, send a message to [log in to unmask] with following text in
>the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt
>or (re-start) delivery of Technet send e-mail to
>[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing
>per day of all the posts: send e-mail to
>[log in to unmask]: SET Technet Digest
>Search the archives of previous posts at:
>http://listserv.ipc.org/archives Please visit IPC web site
>http://www.ipc.org/contentpage.asp?Pageid=4.3.16
>for additional information, or contact Keach Sasamori at [log in to unmask]
>or 847-615-7100 ext.2815
>-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|