TECHNET Archives

November 2010

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Fri, 19 Nov 2010 13:59:38 -0800
Reply-To:
Content-Transfer-Encoding:
7bit
Subject:
From:
John Parsons <[log in to unmask]>
Content-Type:
text/plain; charset="us-ascii"
In-Reply-To:
<933AF4F6E1634B4C894C8837C8A7A94E@ibmmrljzg6xbsk>
Organization:
Enigma Interconnect Inc.
MIME-Version:
1.0
Parts/Attachments:
text/plain (147 lines)
Inge,

The appearance of the PCB land and that of the BGA are the same.  A very
flat, uniform surface, dull grey in colour with, under 45x magnification, a
fine, grainy appearance.  If, under that magnification I touch the pad
surface with an x-acto knife, ever so gently, I can rub off the grainy layer
leaving a shiny silver surface that 'looks' like solder to me.

On hand I have chemistry that will strip tin/lead but apparently it leaves
nickel with a black finish.  I don't have any chemistry that would strip
nickel.

John

-----Original Message-----
From: Inge [mailto:[log in to unmask]] 
Sent: Friday, November 19, 2010 1:25 PM
To: [log in to unmask]; [log in to unmask]
Subject: Re: [TN] BGA Falling off PCA

John,

we have seen this a number of times,and I've been looking at some of these 
cases.You can start with some brief examinations:

1. are there any solder remnants on the board pads. If so, how does it look 
like? Randomly spread or ring formed along the pad's circumperifery?

2.apply a solder etchant that does not etch Nickel to get an opinion about 
the solder wetting

3. apply a nickel etchant that does not etch solder to get an opinion about 
the nickel covering, skip plating, IMC s

4. dispens a 50-100 micrometer solder paste on the failing board pads and 
run through your oven.Wetting, dewetting or non-wetting.

You need a experienced person to do the tests and to interprete the results.

In right hands, often better than pages and pages of EDAX analysis.


Inge


---- Original Message ----- 
From: "John Parsons" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Friday, November 19, 2010 9:31 PM
Subject: [TN] BGA Falling off PCA


>I am not seeing a lot of the usual Friday quiz traffic so I know you
> guys-n-gals are just itching for some real work :o).
>
>
>
> We are a PCB fabricator and one of our customers has returned some
> assemblies to us for feedback.  What they noticed when someone 
> accidentally
> dropped an assembly is that the BGA (352 pin Cirrus Logic EP9312-CBZ) 
> popped
> off the board.  They then proceeded to drop a few more from a height of
> about a foot with the same results.  All the other components on this
> Pb-free assembly stay fast.
>
>
>
> We have received three PCA's and 5 BGA's.  On one of the BGA's a single 
> ball
> has remained on the PCB.  The rest of them all the balls have broken 
> cleanly
> from the PCB leaving a very flat (under x10 magnification) dull gray
> surface.  I sure wish that I could take photo's but lighting is critical 
> and
> I don't think that I have the resources to get photo's that would do 
> justice
> to what the naked eye is seeing.
>
>
>
> Also of note is that the BGA lands are mask defined with a 31mil circuit 
> pad
> and 26mil solder mask relief.
>
>
>
> Does anyone have any ideas as to how we can determine the root cause of 
> this
> failure.  This part has been built for some time but previously the 
> surface
> finish on the PCB was a solder finish.  This is the first run of the 
> boards
> that has an ENIG finish.  This doesn't look to me like a raw board issue 
> but
> that is where everyone looks first isn't it ;o).
>
>
>
> Regards
>
>
>
> John Parsons
>
>
>
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to 
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to 
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16

> for additional information, or contact Keach Sasamori at [log in to unmask] or

> 847-615-7100 ext.2815
> ----------------------------------------------------- 



______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2