TECHNET Archives

July 2008

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Ioan Tempea <[log in to unmask]>
Date:
Fri, 18 Jul 2008 15:35:01 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Igoshev, Vladimir" <[log in to unmask]>
Subject:
From:
"Igoshev, Vladimir" <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (157 lines)
Ioan,

Everything can be broken :-), so I'd have ruled out any handling/processing issues prior to changing the design. Can you establish after what stage they crack?

Regards,


Vladimir

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ioan Tempea
Sent: Friday, July 18, 2008 3:18 PM
To: [log in to unmask]
Subject: Re: [TN] Mechanical damage to BGA

Vladimir,

You have some good points, just like Victor.

The process is leaded and I have no idea when the damage occurs. We've only built 20 pieces, inspected them under the microscope and only realized there is a problem at test.

Under limited investigative resources, I can only say that everything makes me believe the soldering recipe is good enough to create proper joints and that I suspect mechanical action to be the cause.

Therefore I can only rely on this forum's expertise and try to figure out whether this is really an over the edge design, or rather something normal.

If the design is too much, how can it be improved?

If the design is regular stuff, I will put more effort in controlling depanelizing and handling.

Thanks,

Ioan

-----Message d'origine-----
De : Igoshev, Vladimir [mailto:[log in to unmask]] 
Envoyé : July 18, 2008 3:01 PM
À : TechNet E-Mail Forum; Ioan Tempea
Objet : RE: [TN] Mechanical damage to BGA

Hi Ioan,

You didn't specify the type of the joints/process (Pb-free?) and when
the joints fail? Is it right after the SMT and if that is the case, then
what is the cooling rate for the assembly. 

Larger pads could help, of cause (almost any larger thing can carry a
larger load - I'm curious are there going to be any Friday comments on
that statement? :-))

Regards,

Vladimir

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Ioan Tempea
Sent: Friday, July 18, 2008 2:48 PM
To: [log in to unmask]
Subject: [TN] Mechanical damage to BGA

Dear Technos,

 

I have this BGA that gives me a headache. In many instances the boards
do not pass test, we press on the BGA and they start working; a
classic... The problem solder joints are always on the same side of the
component and on the outer row; needless to say, we have a V-groove line
that is manually cracked. So the cause is most likely mechanical stress
that causes the pads to detach from the PCB. After prying off some BGAs
we see the soldering is good, all the pads come off the board and stay
solidly attached to the balls.

 

The specifics of this board are a bit special and I would need your
opinion on what to improve in the design in order to eliminate the
propensity to damage.

 

PCB is 18.55x28.65mm, FR4, 0.55mm [0.021"] thick

The BGA is 17x17mm, 1mm pitch, 0.65mm balls assembled on 0.25mm circular
pads. In the troubled zone the pads are connected to 0.050mm traces.

 

My opinion is that the board flexes very easily and even if we fix the
depanelization (I will modify the panel) all the subsequent handling,
including the integration of this module, puts the joints at high risk.

 

I think the pads are too small so they do not have sufficient adhesive
force to stay put on the PCB. On top of it, the traces are so minute, so
the slightest stress will be destructive.

 

Would increasing the pad size help? Is this construction (thin PCB +
superfine traces) viable?

 

Could the CTE mismatch be strong enough to cause the damage, instead of
the mechanical stress from bending the board?

 

Thank you,

 

Ioan

 

 


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2