Steve,
I just had this problem a short while ago, on through hole capacitor leads.
At first the quality control people were convinced that the holes must be reworked. We
analysed the assembly by X-Ray - luckily it is a small board which could be rotated ,
and saw that the solder stops near one of the inner layers, at more than 50% hole
length.
The X-Ray image showed the hole walls and the solder fill very clearly, as well as the
inner copper layer. Maybe you can try this method.
Gaby
Steve Collins wrote:
> Is there a tool that could be used to check the hole fill after
> wavesoldering. We do not have cross-sectioning capabilities here in the
> plant. I know that IPC calls for 50% hole fill but in our case when our
> quality people on the line see a partially filled hole they try and fill it
> with touching up. we are working on getting a grip on this with some
> difficulty.
>
> As a side note which parameter (% top side heater, dwell time, wave height,
> bottom side temp) on our Soltec wave solder oven would we want to change to
> possibly get greater hole fill when we have a very large heatsink part with
> though hole leads. I really don't have the time this time for a DOE for
> this and was hoping someone else has had this problem.
>
> ##############################################################
> TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
> ##############################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
> the body:
> To subscribe: SUBSCRIBE TECHNET <your full name>
> To unsubscribe: SIGNOFF TECHNET
> ##############################################################
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
> information.
> If you need assistance - contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> ##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|
|
|