TECHNET Archives

February 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Arturo Medellin <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Arturo Medellin <[log in to unmask]>
Date:
Wed, 9 Feb 2005 14:33:48 -0600
Content-Type:
text/plain
Parts/Attachments:
text/plain (81 lines)
 Werner

 Thanks  for your  feedback

 Arturo
----- Original Message -----
From: "Werner Engelmaier" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Monday, February 07, 2005 9:14 PM
Subject: [TN] Re: [TN] Led component Pull  Test


> Hi Arturo,
> I have answered your question inthe past:
> There is no pull test specification. And there is a good reason none
exists.
> First, there cannot be such thing as a real 'lead pull test;' while you
are
> of course pulling on the lead, what you are doing to the solder joint is
> peeling it—the proper reference is a lead-peeling test.
> Second, the solder joint strength, as determined by a lead peeling test,
has
> no bearing on the reliability of the solder joint, provided the peeling
test
> does not reveal inadequate wetting or poor metallization, e.g., 'Black
Pad.'
> Third, in a peeling test you always need to observe the whole peel-load
> history for the whole peeling process; with a 1T or larger heel fillet,
the largest
> load will be at the initial portion of peeling through the heel fillet,
with l
> ower loads subsequently depending on whether or not (or to what extent)
side
> fillets are present.
> Fourth, the fracture surface of the peeled solder joints give typically
more
> information than do the peel-load histories, because the ONLY really
important
> finding is whether or not adequate wetting has taken place, i.e. the
> separation is mostly in the solder vs. being interfacial.
> Fifth, the reliability in actual use does to a large extent depend on the
> heel fillet and the 'bottom flat' wetting; if the foot length is <3W, than
also
> on the presence of a toe fillet, because short feet 'rock' during thermal
> cycling. Side fillets are less important, unless you have wetting
problems.
>
> Regards,
> Werner Engelmaier
> Engelmaier Associates, L.C.
> Electronic Packaging, Interconnection and Reliability Consulting
> 7 Jasmine Run
> Ormond Beach, FL 32174 USA
> Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904
> E-mail: [log in to unmask], Website: www.engelmaier.com
>
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
> -----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2