TECHNET Archives

September 2004

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
"Wenger, George M." <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Wenger, George M.
Date:
Fri, 10 Sep 2004 13:20:08 -0400
Content-Type:
text/plain
Parts/Attachments:
text/plain (115 lines)
Gaby,

the other possibility is that the solder balls happen because the component has extremely poor solderbility.  I'd find out wht the surface finish is on the component and do a solderability test.

Regards,
George

George M. Wenger (908)-546-4531 
Reliability / FMA Engineer
Base Station and Subsystems Group
Andrew Corporation,  40 Technology Drive, Warren, NJ 07059
[log in to unmask]



-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of David D. Hillman
Sent: Friday, September 10, 2004 12:49 PM
To: [log in to unmask]
Subject: Re: [TN] Tin plating on leads HELP!!!


Hi Gaby! Do you know what the component lead surface finish is (what
type/kind of plating)? Some plating types - like bright acid tin plating -
could be the source of the solderballs.  And yes, the 002B surface mount
simulation test would be helpful in determining root cause.

Dave Hillman
Rockwell Collins
[log in to unmask]



                      Gabriela Bogdan
                      <gabriela@NETVISI        To:       [log in to unmask]
                      ON.NET.IL>               cc:
                      Sent by: TechNet         Subject:  [TN] Tin plating on leads HELP!!!
                      <[log in to unmask]>


                      09/10/2004 11:24
                      AM
                      Please respond to
                      TechNet E-Mail
                      Forum; Please
                      respond to
                      Gabriela Bogdan






Dear friends,
After assembly, on all circuits there was one fine pitch PLCC from a
certain vendor which had lots of small solder balls between the leads, even
on the solder mask dam between them.
Other PLCC's with the same pitch were clean.
We tried to see the amount of solder balls by X-ray, and found many more
behind the leads.
At first we thought that our solder paste was the culprit, but seeing that
other components were "normal" , we looked closer to the leads by X-ray,
and saw a lot of small voids only along the leads of the bad component,
these voids reaching to the upper end of the leads, where the solder paste
did  not reach. Visually, the upper part of the leads was very rough.
I suppose that the tin plating of the leads contained additives which epand
during soldering, even burst out, and "spit" the molten solder all around.
If this is the case,how could I reject such components during incoming
inspection?
Should I do a solderability test for each batch on a printed ceramic plate?
Gaby

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

------------------------------------------------------------------------------------------------
This message is for the designated recipient only and may
contain privileged, proprietary, or otherwise private information.  
If you have received it in error, please notify the sender
immediately and delete the original.  Any unauthorized use of
this email is prohibited.
------------------------------------------------------------------------------------------------
[mf2]

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2