Hi Steve,

I can't explain why your bridges are all in the corners, but I do have an idea why some folks are more succesfull than others: are the pads soldermask defined or not ? With soldemask defined pads you'll get a larger stand-off height but less "squishing" then with non soldermask defined pads (see Motorola's application note AN1231). Or maybe these boards have some kind of undefined mixture of SMD and NSMD?  Other factors of influence are size of the pads and the soldermask quality (how good does it prevent solder from flowing over the edge of the pad). With an unlucky combination of these and your metal-plate BGA you have the ingredients for misery.

Kind regards,

Daan Terstegge
Unclassified mail
Personal Website: http://surf.to/smtinfo

>>> "Stephen R. Gregory" <[log in to unmask]> 07/22 2:42 am >>>
This is a subject that has come up before...it has to do with the TI BGA's
with the metal heat sink incorporated into the top of the device. I have
x-ray but it doesn't have enough power to penetrate the heatsink. We've
recently aquired a Ersascope, I've been using that to inspect first article
placement to make sure that we're getting it on the pads...it's been fine.
But we still have had a problem with bridging.

Out of 50 or so boards, there's been maybe 5-6 boards that have bridged. The
bridges have all been in the corners. The balls all seem "squished" because
of the weight of the heatsink. I've been looking closely at everything,
making sure the print is good, placement is accurate, and that my reflow
profile is good too, but I still am seeing this bridging problem...

The last time I brought this subject up, I did get conflicting perspectives
on this problem with the T.I. parts with the heatsinks in them. One
experience shared was that they were having problems processing this part
without bridging, and another perspective was from someone that said they
built many, many boards with this part and didn't have a problem at all...

I'm really trying hard to make sure that everything is as it's supposed to
be, print definition and registration, placement accuracy, and reflow
profile, but I'm still experiencing this bridging problem, 5 or 6 boards out
of 50 isn't good at all...now that I have a Ersascope (because I can't x-ray)
it's painfully easy to see the bridges...and like I said, they're  mostly on
the corners..

Any ideas?

-Steve Gregory-

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################

ATOM RSS1 RSS2