TECHNET Archives

October 2002

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Thu, 31 Oct 2002 07:48:22 -0800
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, "Crepeau, Phil" <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="iso-8859-1"
From:
"Crepeau, Phil" <[log in to unmask]>
Parts/Attachments:
text/plain (133 lines)
hi,

it seems possible in your attempts to get a flat finish on your pads, the hasl people blew off nearly all the solder and left the intermetallics behind.  something like what torpedoed the old oxford process.

phil

-----Original Message-----
From: d. terstegge [mailto:[log in to unmask]]
Sent: Thursday, October 31, 2002 6:32 AM
To: [log in to unmask]
Subject: Re: [TN] HASL process OK or not ?


Hi Mike, 

Yes this was prior to assembly, it's not localised areas of bare copper
but several pads having a dull appearence and a color somewhere between
brown, green, and solder. There's no solder dome, it's very flat.

Daan Terstegge
Unclassified mail


>>> [log in to unmask] 10/31/02 02:23pm >>>
Was there Cu exposed on the bare PWB you inspected, prior to assembly
/
soldering? 

-----Original Message-----
From: d. terstegge [mailto:[log in to unmask]] 
Sent: Thursday, October 31, 2002 6:00 AM
To: [log in to unmask] 
Subject: [TN] HASL process OK or not ?


Hi Technet,

Yesterday I visited one of our bare board manufacturers and had a
close
look at their HASL-process. The reason for the visit was solderability
problems on BGA-pads, which sometimes look thin and dull. Occasionally
copper seems to be visible through the tinlead.
In general I think this is a very professional boardshop, but (being
not an expert) I don't know what to think about their HASL-process. I
hope someone on this great forum is willing to give me some input on
my
findings, in terms of good or bad, or possibilities for improvement:  

Machine: Quicksilver SM, vertical HASL, 250 kg solderpot, no preheat

Time between microetch (drying) and fluxing can be up to two hours

Solder pot temperature set to 255 °C

Leveling is done is such a way that the solder is as flat as possible,
although the design of the airknives causes a big difference betweeen
the two boardsides. With XRF we measured a thickness of only 0.4
microns
on BGA-pads, with about 3 microns on similar pads on the other
boardside.

Water-based flux from an open tank, without any composition control,
but tank is replaced every 24 hours. 
Solder is replaced every 6 months, but except for copper contamination
no composition-check is ever done. 
When copper is above 0.3 % the dross is skimmed off to assure that
copper content stays below 0.35 %.
Throughput of the machine is about 700 panels per day. 

Daan Terstegge
Thales Communications
Unclassified mail
Personal Website: http://www.smtinfo.net 

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV
1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives 
Please visit IPC web site http://www.ipc.org/html/forum.htm for
additional
information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700
ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV
1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives 
Please visit IPC web site http://www.ipc.org/html/forum.htm for
additional
information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2