TECHNET Archives

June 2005

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
text/plain
Sender:
Subject:
From:
"Whittaker, Dewey (AZ75)" <[log in to unmask]>
Date:
Wed, 22 Jun 2005 08:16:18 -0700
MIME-Version:
1.0
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Wenger, George M." <[log in to unmask]>
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, "Whittaker, Dewey (AZ75)" <[log in to unmask]>
Parts/Attachments:
text/plain (458 lines)
Is your mouse pad black?
Dewey

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Wenger, George M.
Sent: Wednesday, June 22, 2005 7:26 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Intermittent Saga, part 2

Richard,

A few minutes is no problem but I got Steve's message at 8:37 and it is now
10:30 and I still can't see them.  For some reason I think the electrons
have slowed down trying to get through our server.

Regards,
George
George M. Wenger
Reliability / FMA Engineer
Base Station and Subsystems Group
Andrew Corporation, 40 Technology Drive, Warren, NJ 07059 (908) 546-4531
[log in to unmask]


-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Stadem, Richard
Sent: Wednesday, June 22, 2005 9:55 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Intermittent Saga, part 2


For those of you who benefit from Steve's website:
I have noticed that there is a little delay before the rest of us can see
the pics, for some reason.
If you do not see new pics right away after he says they are there, just
wait a few minutes and try again.

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Stephen Gregory
Sent: Wednesday, June 22, 2005 8:37 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Intermittent Saga, part 2

Hi George!

Yep, they're up...I just checked.

Kind regards,

-Steve Gregory-
Senior Process Engineer
LaBarge Incorporated
Tulsa, Oklahoma
(918) 459-2285
(918) 459-2350 FAX


|---------+---------------------------->
|         |           "Wenger, George  |
|         |           M."              |
|         |           <George.Wenger@an|
|         |           drew.com>        |
|         |                            |
|         |           06/22/2005 07:44 |
|         |           AM               |
|         |                            |
|---------+---------------------------->

>-----------------------------------------------------------------------
---------------------------------------|
  |
|
  |       To:       "TechNet E-Mail Forum" <[log in to unmask]>,
<[log in to unmask]>                      |
  |       cc:
|
  |       Subject:  RE: [TN] BGA Intermittent Saga, part 2
|

>-----------------------------------------------------------------------
---------------------------------------|




Steve,

Are you sure they are up I can't see them on page 2?

Regards,
George
George M. Wenger
Reliability / FMA Engineer
Base Station and Subsystems Group
Andrew Corporation, 40 Technology Drive, Warren, NJ 07059 (908) 546-4531
[log in to unmask]


-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Stephen Gregory
Sent: Wednesday, June 22, 2005 8:37 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Intermittent Saga, part 2


Good Mornin' Leo and Everyone!

Well, today is starting off really good! (but I just got in...hehehe).

Your two pictures are up Leo. Go to: http://www.stevezeva.homestead.com
and click on Picture Page 2, and look for; "No Nickel Corrosion, and Nickel
Corrosion".

Kind regards,

-Steve Gregory-
Senior Process Engineer
LaBarge Incorporated
Tulsa, Oklahoma
(918) 459-2285
(918) 459-2350 FAX


|---------+---------------------------->
|         |           Leo Higgins      |
|         |           <Leo_Higgins@ASAT|
|         |           .COM>            |
|         |           Sent by: TechNet |
|         |           <[log in to unmask]>|
|         |                            |
|         |                            |
|         |           06/21/2005 11:18 |
|         |           PM               |
|         |           Please respond to|
|         |           TechNet E-Mail   |
|         |           Forum; Please    |
|         |           respond to Leo   |
|         |           Higgins          |
|         |                            |
|---------+---------------------------->
  >
------------------------------------------------------------------------
--------------------------------------|

  |
|
  |       To:       [log in to unmask]
|
  |       cc:
|
  |       Subject:  Re: [TN] BGA Intermittent Saga, part 2
|
  >
------------------------------------------------------------------------
--------------------------------------|





I will send a pair of pictures from an Amkor paper showing optical
micrographs showing Ni corrosion and a pad with no Ni corrosion to Steve to
see if he can put up on his web site.  Published studies on Black Pad issues
often show similar structures.  Steve can you post the 2 photos?
I will send after this note.


Best regards,
Leo

Director of Applications Engineering
ASAT, Inc.
3755 Capital of Texas Highway, Suite 100
Austin, Texas     78704

ph     512-383-4593
fx      512-383-1590
[log in to unmask]
www.asat.com


The information contained in this electronic message is CUSTOMER/SUPPLIER
PRIVILEGED AND CONFIDENTIAL INFORMATION intended only for the use of the
individual or entity named above. If the reader of this message is not the
intended recipient, you are hereby notified that any dissemination,
distribution and copying of this communication is strictly prohibited. If
you have received this communication in error, please immediately notify the
sender by electronic mail. Thank you.



-----Original Message-----
From: [log in to unmask] [mailto:[log in to unmask]]
Sent: Monday, June 13, 2005 2:16 PM
To: [log in to unmask]; [log in to unmask]
Subject: RE: [TN] BGA Intermittent Saga, part 2


You state to look for Au cyanide etching in the eless Ni.   With what
instrument or is this under a high power micro scope (1000X).   Can you
describe what to look for or perhaps you can share a photo of the artifact
you are suggesting.

Victor,

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Leo Higgins
Sent: Monday, June 13, 2005 1:39 PM
To: [log in to unmask]
Subject: Re: [TN] BGA Intermittent Saga, part 2

Excessive stress from pneumatic presses used to bond heat sinks to BGAs
after board level assembly has been shown to induce failure at the solder to
BGA pad on packages that meet pre-SMT assembly quality specs in all ways.
Subsequent analyses may show no evidence of black pad (cross sectioning to
look for Au cyanide etching into the eless Ni, etc.).


Best regards,
Leo

Director of Applications Engineering
ASAT, Inc.
3755 Capital of Texas Highway, Suite 100
Austin, Texas     78704

ph     512-383-4593
fx      512-383-1590
[log in to unmask]
www.asat.com


The information contained in this electronic message is CUSTOMER/SUPPLIER
PRIVILEGED AND CONFIDENTIAL INFORMATION intended only for the use of the
individual or entity named above. If the reader of this message is not the
intended recipient, you are hereby notified that any dissemination,
distribution and copying of this communication is strictly prohibited.
If
you have received this communication in error, please immediately notify the
sender by electronic mail. Thank you.



-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Jana Carraway
Sent: Monday, June 13, 2005 1:01 PM
To: [log in to unmask]
Subject: Re: [TN] BGA Intermittent Saga, part 2


Werner,

If it's black pad on the component side, how would Kerry prove or disprove
it?  Could he find the cause by using Auger or cross-section?
What would be the appropriate tests to perform to find root cause?
Should he send a component back to the supplier for root cause analysis?

Thank you,
Jana Carraway

Jana Carraway
MSEI - Advanced Technology Group
6024 S.W. Jean Road
Lake Oswego, OR  97035
503.697.5291, ext 1180
email: [log in to unmask]

-----Original Message-----
From: TechNet [mailto:[log in to unmask]]On Behalf Of Werner Engelmaier
Sent: Monday, June 13, 2005 10:04 AM
To: [log in to unmask]
Subject: Re: [TN] BGA Intermittent Saga, part 2


Hi Kerry,
You most likely have 'Black Pad' on the componet side. That, together with
the stess concentration from the SMD-geometry, caused a briitle ionterfacial
overstress failure.

Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904
E-mail: [log in to unmask], Website: www.engelmaier.com


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per
day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per
day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per
day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information,
or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per
day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------




__________________________________________________________________
This message may contain information that is privileged and confidential to
LaBarge, Inc.  It is for use only by the individual or entity named above.
If you are not the intended recipient, you may not copy, use or deliver this
message to anyone.  In such event, you should destroy the message and kindly
notify the sender by reply e-mail.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL) To receive ONE mailing per
day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

------------------------------------------------------------------------
------------------------

This message is for the designated recipient only and may contain
privileged, proprietary, or otherwise private information.
If you have received it in error, please notify the sender immediately and
delete the original.  Any unauthorized use of this email is prohibited.
------------------------------------------------------------------------
------------------------

[mf2]




__________________________________________________________________
This message may contain information that is privileged and confidential to
LaBarge, Inc.  It is for use only by the individual or entity named above.
If you are not the intended recipient, you may not copy, use or deliver this
message to anyone.  In such event, you should destroy the message and kindly
notify the sender by reply e-mail.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please visit
IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

----------------------------------------------------------------------------
--------------------
This message is for the designated recipient only and may contain
privileged, proprietary, or otherwise private information.
If you have received it in error, please notify the sender immediately and
delete the original.  Any unauthorized use of this email is prohibited.
----------------------------------------------------------------------------
--------------------
[mf2]

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in the
BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet
NOMAIL or (MAIL) To receive ONE mailing per day of all the posts: send
e-mail to [log in to unmask]: SET Technet Digest Search the archives of
previous posts at: http://listserv.ipc.org/archives Please visit IPC web
site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2