I think you have entered the strange zone of dewetting, which is not the
same as non wetting.
It is quite possible that something has changed to allow poor or
marginal initial wetting, which on re-exposure causes non wetting. It
would be interesting to see what happens if you simply double the
initial exposure time - you might then go straight to non wetting.
Dewetting is usually, but not always a function of some sort of
contamination.

Regards 

Mike Fenner 
Indium Corporation 

T: + 44 1908 580 400
M: + 44 7810 526 317 
F: + 44 1908 580 411 
E: [log in to unmask] 
W: www.indium.com 
Pb-free: www.Pb-Free.com 



-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Braddock, Iain
Sent: 08 April 2004 15:54
To: [log in to unmask]
Subject: Re: [TN] Strange phenomenon!


Thanks Werner,

The reflow temperature measured at the lead I/F is 215C. These boards
have
been built for the last 2 years without this problem but now there is.


If the joints are rerun with a soldering iron the problem goes away but
this
is a cumbersome, non value added activity which I am trying to address.

I am considering having the failed joints analysed by one of the
universities that specialise in Auger / SIM microscopy.

Regarding your last comment, if the lead / foot wasn't solderable at all
would you expect the formation of a joint ie. a nice meniscus as we
have,
though obviously a weak metallurgical bond I wouldn't have thought so!

Regards,
        Iain.

-----Original Message-----
From: Werner Engelmaier [mailto:[log in to unmask]]
Sent: 08 April 2004 13:05
To: [log in to unmask]
Subject: Re: [TN] Strange phenomenon!


               *** WARNING ***

This mail has originated outside your organization,
either from an external partner or the Global Internet.

     Keep this in mind if you answer this message.


Hi Iain,
Remember, that what you are soldering to in Alloy 42 is the 42% nickel
in
it.

As such you need to raise the reflow temperature some 15 to 20°C over
what
is

needed for Cu.

Also, there occasionally apppears   Allloy 42 that is   not solderable
at

all; thus, your gullwing feet are simply encased in solder without any

metallurgical bond.

Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737
E-mail: [log in to unmask], Website: www.engelmaier.com

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send


:::::::::::::::::::::::::::

This email, its content and any files transmitted with it are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient please delete and contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination or other use of, or taking of any action in reliance upon, this information by persons or entities other than the intended recipient is prohibited.

Messages sent via this medium may be subject to delays, non-delivery and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. In particular, Indium Corporation does not accept responsibility for changes made to this email after it was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.

:::::::::::::::::::::::::::

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2