Curious, why do some end users make comments about finding new suppliers
when assemblers ask questions about probable board defects?

Just curious is all, consider I notice this on some e-mail replies.

Thanks,

Franklin

----- Original Message -----
From: Kasprzak, Bill (esd) USX <[log in to unmask]>
To: <[log in to unmask]>
Sent: Wednesday, November 10, 1999 12:44 PM
Subject: Re: [TN] Voids after Wave-Soldering!


Paul:

Anytime I've seen volcanic type voids as you have described generally points
to moisture trapped inside the board near the plated thru hole. Try baking a
board for a couple of hours at 225° - 250°F, then re-run. If the problem
persists then all I can say is that there are volitiles trapped inside your
PWB and nothing can be done to remove them except to talk to your board
supplier. (or find a new one !)

Bill Kasprzak
Moog Inc.
> -----Original Message-----
> From: Paul Tomlinson [SMTP:[log in to unmask]]
> Sent: Wednesday, November 10, 1999 10:57 AM
> To:   [log in to unmask]
> Subject:      [TN] Voids after Wave-Soldering!
>
> Hi folks,
>
> I am just learning about these matters, and this is THE place where
> knowledge and experience abounds so please somebody help me with this.
>
>
> I have just had my first ever boards waved and the results are not
> encouraging.  What could be the cause of a volcano shaped void between the
> component leads being soldered and the main body of the solder?
>
>
> There is perfect continuity, the area at the tip and that around the board
> are well wetted, but mechanically the joints are very weak and prone to
> failure, the parts can actually be pulled out of the board without being
> damage.
>
>
> Could this be simply the result of a too low temperatured wave?  They used
> 465F.
>
>                        |       |
>                        |       |
>                        |       |
> --------------------- |       | -------------------
>                      | |       | |
>                      | |       | |
>                      | |       | |
> --------------------- |       | -------------------
>            *         * |       |  *         *
>           *         *V |       | V *         *
>            *       * O |       | O  *       *
>             *      * I |       | I  *      *
>               *    * D |       | D  *    *
>                 *   *  |       |   *   *
>                   *  * |       |  *  *
>                     * *|       | * *
>                      * |       | *
>                       *|       |*
>                        ---------
>
> This ASCII art is extremely crude so I have attached both JPG and BMP
> files
> of a much better drawing.
>
> Tia,
>
> Paul. << File: lead.bmp >>  << File: lead.jpg >>  << File: ATT15807.txt >>
>

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following
text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################

##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe:   SUBSCRIBE TECHNET <your full name>
To unsubscribe:   SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################

ATOM RSS1 RSS2