TECHNET Archives

July 2010

TechNet@IPC.ORG

Options: Use Proportional Font
Show HTML Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Paul Reid <[log in to unmask]>
Reply To:
TechNet E-Mail Forum <[log in to unmask]>, Paul Reid <[log in to unmask]>
Date:
Thu, 15 Jul 2010 17:30:48 -0400
Content-Type:
text/plain
Parts/Attachments:
text/plain (281 lines)
Hi Werner,

Yes, we have had this discussion. 

I apologies for the use of the term "live steam" but that is an understandable example of vapor pressure.

I believe that Dr. Rothschild is correct; the volume of water counts, a small volume of water has limited ability to produce pressure compared to a large volume of liquid water in the same container. At some point you run out of water and the pressure is limited. The pressure still increases, with increased temperature, but only as a function of increasing the speed of the molecules, not adding molecules as we see with vapor pressure. After water condensed in the voids in the PWB or absorbed in the epoxy has evaporated there is no vapor pressure, just gas pressure, acting as per the ideal gas laws (thank you Bob Kondner). You notice no one is talking about the pressure exerted in the PWB by nitrogen. Nitrogen is not in a "vapor pressure" relation within the board. I don't know if this is the correct way to express myself.

"Vapor pressure or equilibrium vapor pressure are the pressure of a vapor in thermodynamic equilibrium with its condensed phases in a closed bottle". You notice the word "equilibrium" is used. This is what I think Wayne was pointing out when he says there is a limit based on amount.

Other comments for all ...

We cannot objectively demonstrate an increase in reliability of the board that is significant with or without a bake if the board is well manufactured etc. We have improved reliability by baking if the board was under cured. We have degraded the reliability by baking too long and too high a temperature. 

I believe baking stress relieves the board and drives out moisture but rarely is that enough to affect a significant reliability improvement in either extending cycles to failure were copper is the failure mode, or reducing material damage where material degradation is the dominant failure mode. 

Many times, this year we have baked coupons that are prone to delamination. Baked and unbaked coupon showed the same tendency to delamination and failed electrically at the same rate.

We measure material damage by changes in capacitance. Measuring picofarads, a 4% change in capacitance on our test coupons reflect material damage that is visible by microsectioning. Coupons with a 4% change in capacitance may exhibit and artificial extension of cycles to failure. With this method we find the material damage that is not visible by macroscopic examination. Using capacitance allow us an increased acuity of material damage and insight to PWB reliability.  


Sincerely, 
Paul Reid 

Program Coordinator 
PWB Interconnect Solutions Inc. 
235 Stafford Rd., West, Unit 103 
Nepean, Ontario 
Canada, K2H 9C1 
613 596 4244 ext. 229 
Skype paul_reid_pwb 
[log in to unmask] <mailto:[log in to unmask]> 


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Werner Engelmaier
Sent: July 15, 2010 3:01 PM
To: [log in to unmask]
Subject: Re: [TN] BAKING OF PWB QUESTION

 Hi Paul,
I think we went over the water vapor/steam issue once before.
It simply is not so that one needs liquid water to have an increase in pressure.
Consider a closed vessel with some water in it. As you heat the vessel the liquid water will vaporize until all of it has vaporized. Just because you no longer have liquid H2O does not mean that the pressure does not increase with increasing T-you now have superheated steam that follows the equation P= RT/V-so the higher the temperature the higher the pressure for a constant volume. V certainly can increase with delamination and some of the superheated steam will escape. The term 'live steam' has no meaning in this context-its primary use is for model railroading, and refers to steam actually doing some work in driving the locomotive. Inside the PCB, liquid water per se does hardly ever exist, the steam does do 'work' only in terms of increasing the internal vapor pressure, and you certainly do not need liquid water for that.
Werner

 


 

 

-----Original Message-----
From: Paul Reid <[log in to unmask]>
To: [log in to unmask]
Sent: Thu, Jul 15, 2010 11:37 am
Subject: Re: [TN] BAKING OF PWB QUESTION


This is a good thread. 



Off-line Ian Hanna from Circuit Tech comments:  



"Hey Paul,  I would expect that the biggest threat from trapped moisture is the 

vapour pressures generated during the initial shock of assembly...would this be 

visible during cyclic reliability testing?  Regards - Ian"



The answer to Ian's question is, yes, the greatest "threat" (or at least 

pressure) from trapped moisture is during the initial thermal excursion and yes 

it is visible during reliability testing. But no we do not see delamination 

during the first thermal cycle and if the material delaminates the effect is 

extended cycles to failure. The lesson is you have to test both the copper and 

the material when doing reliability testing for lead/free applications incase 

the material degrades and you get false positives from thermal cycle testing. We 

measure material damage by means of changes in capacitance in representative 

coupons in order to capture material damage.



Basically we are saying that many studies demonstrate limited impact, positive 

or negative, on reliability due to baking. Dr. Taube shows "moisture in" or 

"moisture out" has a limited reliability affect. The effect of baking is not 

compelling for extending ability to survive assembly and rework.



The idea is that vapor pressure from trapped water "blows" the material apart. 

It is my contention that if the adhesion between laminated surfaces is weak, by 

that I mean, between B-stage and C-stage or B-stage and copper, then vapor 

pressure generated from trapped water may cause frank delamination. But there is 

more to this story.



I expect the greatest pressure from water vapor would occur during heating on 

the first thermal excursion because the board has the greatest amount of water 

at the beginning of assembly. After the first cycle moisture must have been out 

gassing during the thermal excursion. The longer at temperature the less water 

in the board so by the second thermal excursion there should be less pressure 

because some of the water has been lost. Our findings are consistent with Dr. 

Taube's findings. Delamination does not typically occur on the first thermal 

cycle. Delamination frequently occurs after the third thermal excursion. Let's 

let that stand for a second.



Dr. Wayne Rothschild points out that the vapor pressure is limited by the amount 

of water available to the system. He points out that the gas laws take into 

account the amount of water in the system.



Pressure increases rapidly with "live steam" but, when the water is all 

vaporized, the pressure increase is reduced. "Live steam" requires liquid water 

as a source to replace the steam. A steam train stops when it runs out of water. 

The vapor pressure goes to zero once the water escapes out of the board. 



So bringing Dr. Taube's and Dr. Rothschild's observations, our experience in 

reliability testing, and how samples fail in T260 testing on a TMA,  together, I 

feel that the damage to material is from vapor pressure, z-axis expansion and 

also material degradation. The epoxy system is failing and volatiles are 

providing a force as is z-axis expansion of the epoxy system, to a point were 

force is greater than the strength of the epoxy and the board fails. Epoxy 

degradation is a major component of the failures and aggressive baking could 

degrade the epoxy reducing reliability in a lead/free application.



All this stands given that the copper is not being degraded by 260°C, which I, 

and others are beginning expect it is changing, when the copper is poorly plated 

and of a lower quality. But that is another story. 







Sincerely, 

Paul Reid 



Program Coordinator 

PWB Interconnect Solutions Inc. 

235 Stafford Rd., West, Unit 103 

Nepean, Ontario 

Canada, K2H 9C1 

613 596 4244 ext. 229 

Skype paul_reid_pwb 

[log in to unmask] <mailto:[log in to unmask]> 





______________________________________________________________________

This email has been scanned by the MessageLabs Email Security System.

For more information please contact helpdesk at x2960 or [log in to unmask] 

______________________________________________________________________



---------------------------------------------------

Technet Mail List provided as a service by IPC using LISTSERV 15.0

To unsubscribe, send a message to [log in to unmask] with following text in

the BODY (NOT the subject field): SIGNOFF Technet

To temporarily halt or (re-start) delivery of Technet send e-mail to 

[log in to unmask]: SET Technet NOMAIL or (MAIL)

To receive ONE mailing per day of all the posts: send e-mail to 

[log in to unmask]: SET Technet Digest

Search the archives of previous posts at: http://listserv.ipc.org/archives

Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for 

additional information, or contact Keach Sasamori at [log in to unmask] or 

847-615-7100 ext.2815

-----------------------------------------------------


 

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2