Rich,
Electroless nickel (EN) plating is generally solderable until the phosphor
content in the plating exceeds 5-7 percent. (H. Manko, Solders and
Solderability)
However, solderability may be adversely affected in EN platings with as low
as 3.5% percent phosphor content if the plating has been subjected to heat
treating. (B. Dunn, Metallurgical Assessment of Spacecraft Parts, Materials
and Processes)
Tin-lead solder tinning of electroless nickel plated copper wire can be
accomplished successfully at +725-750F with RMA or RA flux.
Bob
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Richard Kraszewski
Sent: Friday, May 27, 2005 8:11 AM
To: [log in to unmask]
Subject: [TN] Solderablity of ElectrolessNickel
I'm trying to clearly confirm the level of phosphorus at which the
solderability of electroless nickel starts to be severely reduced.
Traditionally, I always thought it was 5%. I colleague of mine claims
that he's got a paper from 89' at the "Electroless Ni Conference" that
states that up to 3% is no problem. I do recall seeing an article last
year where 6 to 8% seems to be the preferred maximum .
Any thoughts on what the appropriate level should be, and/or the
mechanism of why it is it degrades solderablity would be truly
appreciated.
Rich K - KEDS
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|