TECHNET Archives

March 2011

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Joyce Koo <[log in to unmask]>
Date:
Tue, 22 Mar 2011 14:04:22 +0800
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Lum Wee Mei <[log in to unmask]>
Subject:
From:
Lum Wee Mei <[log in to unmask]>
Content-Transfer-Encoding:
base64
In-Reply-To:
Content-Type:
text/plain; charset="UTF-8"
MIME-Version:
1.0
Parts/Attachments:
text/plain (1 lines)
Sorry, I am lost in translation. What is HOP?

Regards,
~wee mei~


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Joyce Koo
Sent: Monday, March 21, 2011 11:48 AM
To: [log in to unmask]
Subject: Re: [TN] Query on failure of assembled PCB

Look a bit skimpy on Au to me.  HOP possibly is my guess for the fault (if it is, buy me a cup of coffee.  Pete's will do:-), consider Ni-oxide is not easily solderable.   
--------------------------
Sent using BlackBerry


----- Original Message -----
From: Uppina Nagaraj [mailto:[log in to unmask]]
Sent: Sunday, March 20, 2011 11:33 PM
To: [log in to unmask] <[log in to unmask]>
Subject: Re: [TN] Query on failure of assembled PCB

Hi,

Ni is around 3.9~5 microns & Au is around 0.07 to 0.10microns.

Thanks!
U.Nagaraj


> How thick is the ENIG?
>
> Victor,
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Wenger, George M.
> Sent: Wednesday, March 16, 2011 10:43 PM
> To: [log in to unmask]
> Subject: Re: [TN] Query on failure of assembled PCB
>
> U.Nagaraj
>
> Chris and Joyce have suggested good possibilities.  The intermittent
> failures could be brittle solder joint fractures at BGA ball / PCB pad
> interface or they could be HOP failures.  If the boards really do work
> immediately after they are built but are intermittent a couple of weeks
> later and they have not been under any mechanical stress then HOP might be
> the cause.  With HOP you might get enough contact immediately after
> soldering to pass test but as the solder surfaces oxidize the contact
> resistance could increase causing intermittent failures.
>
> Regards,
> George
> George M. Wenger
> Senior Principal Reliability / FMA Engineer
> Andrew Corporation - Wireless Network Solutions
> 40 Technology Drive, Warren, NJ 07059
> (908) 546-4531 Office (732) 309-8964 Mobile
> E-mail: [log in to unmask]
>
>
> -----Original Message-----
> From: Joyce Koo [mailto:[log in to unmask]]
> Sent: Wednesday, March 16, 2011 11:20 PM
> To: [log in to unmask]; Wenger, George M.
> Subject: Re: [TN] Query on failure of assembled PCB
>
> One major difference: the exit test is possibly connectivity test: open or
> short, not function.  The BGA intermittent is a functional test.  You
> could pass open or short, but still got intermittent fault.  HOP may pass
> open short test if it got some contact, sounds like either bga cracked, or
> hOP,or microvia cracked.  All of them will exhibit intermittent but
> partially show connectivity when apply pressure. Are those parts
> underfilled?
> --------------------------
> Sent using BlackBerry
>
>
> ----- Original Message -----
> From: Wenger, George M. [mailto:[log in to unmask]]
> Sent: Wednesday, March 16, 2011 10:42 PM
> To: [log in to unmask] <[log in to unmask]>
> Subject: Re: [TN] Query on failure of assembled PCB
>
> U.Nagaraj
>
> What was the PCB surface finish?
>
> Regards,
> George
> George M. Wenger
> Senior Principal Reliability / FMA Engineer
> Andrew Corporation - Wireless Network Solutions
> 40 Technology Drive, Warren, NJ 07059
> (908) 546-4531 Office (732) 309-8964 Mobile
> E-mail: [log in to unmask]
>
> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]] On Behalf Of Uppina Nagaraj
> Sent: Wednesday, March 16, 2011 10:28 PM
> To: [log in to unmask]
> Subject: [TN] Query on failure of assembled PCB
>
> Dear All,
>
> 1. We are manufacturers of PCBs. One of our customer has reported
>    failure in assembled boards. The main observation is that after
>    assembly, the assembled units were functioning normally
>    and had passed all the stipulated electrical tests. These parts
>    were kept at the assembly house for around over 3-4 months. Later
>    when the assembled units were scheduled to be integrated into
>    the system, the assembled units were tested again, but now they
>    see failure.
>
>     These are the inputs given to us..........
>     a) Failures are intermittent in nature.
>     b) Failures are concentrated in and around the area where
>        BGA is mounted.
>     c) Some failures are recovered by applying mechanical stress on
>        the PCB.
>     d) Some are recovered by subjecting to reflow.
>     e) There are no component failures.
>
> 2. Our customer's assembly process flow is…
>     a) 100Deg C, 16 hours baking
>     b) Assembly done within 24 hours after baking
>     c) Pb-free reflow conducted with a peak temperature of 262Deg C
>     d) Reflow is done 2 times (once for each side of components)
>     e) Visual and physical inspection done
>     f) Cycling done at -20~+70Deg C for 10 cycles. First 9 cycles
>        are 30minutes per cycle and the last cycle is 1 hour cycle
>    g) Electrical testing
>
> 3. We had retrieved a blank PCB from the same batch and conducted
>    the following trial......
>
>    a) A standard step of baking prior to assembly (100Deg C,
>       16 hours baking) was skipped due to time constraint.
>    b) 2x reflow done at customer's place using standard profile
>       used for assembly of this part.
>
>      Electrical Testing (BBT) on bare PCB passed .
>
>    c) 10 cycles of temp. cycling done at customer's place using the
>       standard cycling profile used for assembled unit.
>
>       Electrical Testing (BBT) on bare PCB passed .
>
>    d) Repeated 2x reflow (2nd time) at customer's place using
>       standard profile used for assembly of this part.
>
>       Electrical Testing (BBT) on bare PCB passed .
>
>      Based on the above trial, we feel that the failure seen is
>      not due to PCB failure.
>
>
> 4. This particular PCB is a 8 layer PCB, built using ISOLA FR370HR
>    material.
> -----------------------------------------------------------------
>
>
> Please share your inputs and thoughts on the failure phenomenon and
> how to ascertain if the failure is due to PCB or assembly.
>
> Thanks in advance!
>
> Best Regards,
> U.Nagaraj
>
>
>
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 15.0
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site
> http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100
> ext.2815
> -----------------------------------------------------
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ---------------------------------------------------------------------
> This transmission (including any attachments) may contain confidential
> information, privileged material (including material protected by the
> solicitor-client or other applicable privileges), or constitute non-public
> information. Any use of this information by anyone other than the intended
> recipient is prohibited. If you have received this transmission in error,
> please immediately reply to the sender and delete this information from
> your system. Use, dissemination, distribution, or reproduction of this
> transmission by unintended recipients is not authorized and may be
> unlawful.
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>
> ______________________________________________________________________
> This email has been scanned by the MessageLabs Email Security System.
> For more information please contact helpdesk at x2960 or [log in to unmask]
> ______________________________________________________________________
>



______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/ContentPage.aspx?Pageid=E-mail-Forums for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

ATOM RSS1 RSS2