Greg:
You are clearly having a problem with oxide formation. The tarnish on the traces is inhibiting the alt oxide formation.
Perhaps the easiest immediate answer is to first dump, then increase the water flow in rinses after Cupric etching. The oxide is probably coming from Copper/Chloride contaminated rinses.
At risk of proposing the unthinkable, you may want to consider a different alkaline cleaner, one that is designed to remove oxide also. Should you need a source for such a product, just ask... :-)
Rudy Sedlak
RD Chemical Company
Greg Triggs <[log in to unmask]> wrote:
Hello
I know that there are not a lot of Fab Guys still out
there, but here goes. Over the years I have seen a problem with coverage
of the oxide replacement along the traces when the layers have been etch
using cupric rather than alkaline. What you see is a lack of coverage on
the fine traces with full coverage on the larger lines and ground
planes. The coverage problem is worse as the copper weight gets higher.
This seems to point to a problem that begins in the cupric etcher, and
becomes worse the longer the layer is in the etcher. If the layers are
passed thru a chem clean (acid) prior to oxide replacement the problem
goes away. Typical clean prior to oxide replacement is alkaline (dryfilm
residue). This seems to indicate that whatever is on the edge of the
trace is acid soluble. Most people seem to blame the dryfilm strip
process, but the isolated lines and ground planes don't have the
problem. I would appreciate any input. Thanks.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------
You snooze, you lose. Get messages ASAP with AutoCheck
in the all-new Yahoo! Mail Beta.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|