I don't agree that the temperature has much to do with the factors that determine the ability to etch extremely fine lines: yes it will influence the rate of etching, but if the spray at all nozzles is at the same temperature (a given) then then I don't see the benefit in going crazy with temperature control more accurate than +/-1 degree.
To Rudy's points about SG control: I agree with the need to control pH. However controlling the metal by SG alone is impossible as the chloride molarity affects density directly. In other words, what you are measuring witha SG controller is the combination of metal content plus Chloride molarity.
So that leaves real-time metal analysis as the only way to control metal concentration which would be impractically expensive.
Peter Blokhuis
Edward Szpruch <[log in to unmask]> wrote:
Rudy,
Two additional points, both of crucial importance :
- tight control of temperature
- tight control of spray pressures ( upper and lower spray , across etching chamber and real exact jobs - post etch spray nozzles )
Regards
Edward
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of R Sedlak
Sent: Wednesday, September 13, 2006 12:01 PM
To: [log in to unmask]
Subject: [TN] Ammoniacal Etch
Joe, Wayne, and others...
A couple of words about ammoniacal etch which might help shed some light on the situation.
90+% of the pcb fabricators control ammoniacal etch using only density (Baume').
This was adequate when we called 10 mil line and space "fine lines", but really is not adequate for today's world...
Think about the fact that Cupric etch has three conditions which are monitored:
Metal content (By density)
Acidity (Usually by conductivity)
Cuprous Content (By ORP)
If you were going to control ammoniacal with the same precision you would control by the following
Metal Content (By density)
pH (Comparable to Acidity in the Cupric etch)
Cuprous Content (which is controlled by air flow through the chamber)
So, in many ways the ammoniacal etch today could be considered to be operating on luck. The system works best when it is used continuously. The system is pushed to its limits when operated intermittently.
Rudy Sedlak
RD Chemical Company
---------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
Yahoo! Messenger with Voice. Make PC-to-Phone Calls to the US (and 30+ countries) for 2¢/min or less.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
How low will we go? Check out Yahoo! Messenger’s low PC-to-Phone call rates.
|
|
|