TECHNET Archives

April 2005

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Date:
Sat, 16 Apr 2005 09:45:43 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Vladimir Igoshev <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="UTF-8"
From:
Vladimir Igoshev <[log in to unmask]>
Parts/Attachments:
text/plain (84 lines)
Hi Donald,

There is one more thing not to be forgoten - component plating and it could (and sometimes does, but don't ask me why) have enough gold to cause the problem.

Vladimir
Sent from my Blackberry Wireless 
Vladimir Igoshev, 519-888-7465 ext.5283


-----Original Message-----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Sat Apr 16 09:32:17 2005
Subject: [TN] ENIG Gold Embrittlement

I have heard a lot of differing views about Gold Embrittlement lately here 
and I am curious, has anyone here found evidence that ENIG causes this?

 From what I have read, the ENIG process lays down about 120 to 240 micro 
inches of Ni and 2 to 4 micro inches of Au.

If you calculate the percent by weight of Au in the solder joint, you have 
to have a very very thin stencil to even come close to having a problem 
with the Au.

I have seen the following data from several different sources and most 
recently in a workshop presented by George Milad and Donald Gudeczauskas of 
Uyemura International Crop at APEX this past February. Their data shows 
that with a 5-mil stencil and a Au thickness of 20 micro inches, the 
percent of Au in the solder joint is 1.54%. Now of course, you are not 
going to get 20 micro inches out of this immersion process and even if you 
plated the Au, this is just at or below the threshold for Au embitterment.

So with a nominal thickness of say 5-micro inches of Au and a 5-mil 
stencil, the percent by weight of Au in the solder joint would be 0.38%. 
Would this be a problem? I don't think so. So has anyone evidence that it does?

Below are just two of many sites talking about gold embrittlement. These 
have some neat pictures to go along with the text.

<http://www.npl.co.uk/ei/documents/gold.pdf>http://www.npl.co.uk/ei/documents/gold.pdf

http://www.alphametals.com/products/solder_solutions/pdf/soldergld.pdf




Donald Kyle C.I.D.+
281-285-7528 voice
281-285-8593 fax
[log in to unmask]
Schlumberger
Sugar Land Product Center (SPC)
Mail Drop MD155-1
155 Industrial Boulevard
Sugar Land, Texas 77478 


---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------




---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2