Hi All!
Maybe some of you remember quite a while back, I had a problem with some
boards with the soldermask flaking off all the copper after 3-cleanings in
our MCS-1000. It's basically a fancy-smancy batch cleaner. We use Kyzen
Aquanox XJN at between a
25-30% concentration (recommended by Kyzen). We also run our wash temps at
140º F., and our rinse at 120º F.
Back when it happened last time we narrowed things down to the soldermask not
being able to take the Aquanox, it was a dry-film (Dynachem Dynamask). We had
other boards that had dry-film on them that we built and showed no
ill-effects from the cleaning. I looked into things and learned that these
boards were masked with a Dupont 8100 series dryfilm...so made it a point to
specify Dupont dry-film on the boards that require dry-film.
Well guess what? I'm starting to see the problem again. Our fab vendor swears
up and down they used a Dupont dry-film. What I see, is that after the second
wash the mask will start to "bubble" and lift on the vias (and sometimes the
traces too), the film hasn't broken yet (it's still intact, it appears to
just be lifting from the copper), but after you wash the board the third
time, the mask starts flaking off all the copper... vias, traces, everywhere.
So I guess I'm starting to wonder now if it's really a mask compatibility
issue with the Aquanox, or is it possibly something about the quality of the
surface prep prior to solder masking?
Have any of you seen this before?
Thanks!
-Steve Gregory-
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|
|
|