BSOB is also called "stand-off stitch". Not what we have here.
What we have here is how the designer solved a problem where two connections had to be done to a single die pad. I've seen that done with a multi-stitch ball bond (much more common with wedge bonds), but very few bonders support that profile. So this designer elected to simply stack two balls.
The weak point is the weld between the ball on top and the wire/ball it's being stacked on. While it is frequently dismissed as "it's a gold to gold bond, so anything goes" I have found failures. The problems with making them reliable are:
1. Ball bonders are nearly always used in "thermosonic" mode, with an emphasis on the "sonic". Most of the weld energy comes from the ultrasonic scrubbing. But with the fully annealed soft gold ball, it is hard to get reliable scrub--even without the fact that the surface being welded to is so irregular.
2. There is no simple way to qualify such a bond. Ball bonds are typically qualified by shear test because the weld area is much larger than the wire area (a pull test should always fail in the wire). But this stacked structure doesn't lend itself to shear testing. So the tech has no way of setting up the bonder to get statistically relevant results without doing thousands of bonds.
Despite these two misgivings, everyone who bonds complex assemblies ends up doing this occasionally and they seem to have a reasonable service life. And they are allowed as repairs for US mil spec parts (not sure about space qual).
Wayne Thayer
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Joyce Koo
Sent: Wednesday, October 27, 2010 10:23 AM
To: [log in to unmask]
Subject: Re: [TN] Unusual Au ball bond
Try google wirebond BSOB (not a bad word).
--------------------------
Sent using BlackBerry
----- Original Message -----
From: Steve Gregory [mailto:[log in to unmask]]
Sent: Wednesday, October 27, 2010 10:13 AM
To: [log in to unmask] <[log in to unmask]>
Subject: Re: [TN] Unusual Au ball bond
Hi Vict..I mean, "X",
Here's your pictures:
http://stevezeva.homestead.com/X-sec-1c.JPG
http://stevezeva.homestead.com/X-sec-1g.JPG
It looks like they wanted to be double sure that it worked ;^)
Steve
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Victor Hernandez
Sent: Wednesday, October 27, 2010 9:01 AM
To: [log in to unmask]
Subject: [TN] Unusual Au ball bond
Fellow TechNetters:
Has anyone seen a ball bond as suck and is it reliable? Photo was sent
to Steve Gregory.
"X"
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential information, privileged material (including material protected by the solicitor-client or other applicable privileges), or constitute non-public information. Any use of this information by anyone other than the intended recipient is prohibited. If you have received this transmission in error, please immediately reply to the sender and delete this information from your system. Use, dissemination, distribution, or reproduction of this transmission by unintended recipients is not authorized and may be unlawful.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
This e-mail and any files transmitted with it may be proprietary and are intended solely for the use of the individual or entity to whom they are addressed. If you have received this e-mail in error please notify the sender.
Please note that any views or opinions presented in this e-mail are solely those of the author and do not necessarily represent those of ITT Corporation. The recipient should check this e-mail and any attachments for the presence of viruses. ITT accepts no liability for any damage caused by any virus transmitted by this e-mail.
______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|