TECHNET Archives

September 2011

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>
Date:
Wed, 14 Sep 2011 12:03:40 +0200
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Cedric ORAIN <[log in to unmask]>
Message-ID:
<046101cc72c5$954cbda0$bfe638e0$@[log in to unmask]>
Subject:
From:
Cedric ORAIN <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (142 lines)
Hello REX,

Thanks for sharing. Do you confirm you have SMD process with SAC alloy using
Sn100C fichich ?

Regards,

Cedric 

-----Message d'origine-----
De : TechNet [mailto:[log in to unmask]] De la part de Rex Waygood
Envoyé : mercredi 14 septembre 2011 10:21
À : [log in to unmask]
Objet : Re: [TN] Sn100C

I am quite surprised that you had a problem with HAL/HASL SN100C.
We allow HASL of SN100C/SACX/SAC and the various combinations of SnCu
that are on offer and I don't recall a solderability issue since RoHS
day (-1 year!). We process lots and lots of boards with these finishes.
I wish ENIG were as trouble free.
We solder with SN100C in our solder bath and it has been a fairly
painless transition from a SAC alloy that we originally used. 

Regards
Rex

Rex Waygood
Technical Manager
 
Hansatech EMS provides value manufacturing through engineering and
quality
 
Hansatech EMS Limited
Benson Road
Nuffield Industrial Estate
Poole
Dorset
BH17 0RY
 
+44 (0)1202 338200


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Cedric ORAIN
Sent: 14 September 2011 08:20
To: [log in to unmask]
Subject: [TN] Sn100C

Good morning again !

 

This is the second subject for which I need your help today. During
previous work -when I qualified lead free assembly years ago- several
PCB finitions was compared. Among the finitions we tested, HAL Sn100C
was rejected because of reflow issues using SAC305 solder paste. 

 

Problems were lack of solderability. I assumed that the reason was
because of the difference between liquidus of Sn100c in comparaison with
SAC305. We didn't make a lot of work to solve that as we head quickly to
ENIG and I finally rejected Sn100C. until this week when a customer
request Sn100C for cost reason.

 

So I would appreciate testimony of technetters that use successfully
Sn100C as PCB finition with SMD process as well as troubleshooting
feedback regarding this process.

 

Regards,

 

Cedric

 <http://www.inovelec-group.com> www.inovelec-group.com

 

 



______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or
[log in to unmask]
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0 To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives For
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

______________________________________________________________________
This email has been scanned by the MessageLabs Email

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2