Russ:
It does sound like your bath is plating out. Probably too much chemistry and
or not enough panel plating. An overactive bath will start to plate the
walls of the tank.
Also the bath may have dropped off in which case you need to remake a new
one.
We generally transfer our electroless bath on a routinely basis from one
tank to another especially in summer. In winter we have a heater that is
turned on in the morning and once it reaches room temp it is turned off. In
summer it is not turned on at all.
Transferring off the bath is a must in order to remove any plate outs or
sediments. Air agitation is a must or else the bath will plate out.
Hope this helps.
Sona Sitapara
Fineline Circuits Inc.
----- Original Message -----
From: "Russell Burdick" <[log in to unmask]>
To: <[log in to unmask]>
Sent: Thursday, January 15, 2004 3:39 PM
Subject: [TN] eless copper
> Hello everybody,
>
> Today's chemistry question concerns electroless copper plating.
>
> Problem is small nodules of copper deposited on the surface of the board
and
> in the holes at the electroless copper bath. Noticable differences in bath
> operation is more foaming during plating and more foam present after
plating
> is completed. Also, a noticable black/dark green particulate visible on
the
> foam surface and eventually on the tank wall and equipment.
>
> Have previously found and corrected excessive EDTA conc. ( indicating
higher
> than wanted proprietary bath chemicals ). Problem still exists but to a
> lesser extent.
>
> Thanks for all help.
>
> Russ
>
> _________________________________________________________________
> Let the new MSN Premium Internet Software make the most of your high-speed
> experience. http://join.msn.com/?pgmarket=en-us&page=byoa/prem&ST=1
>
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
> -----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------
|
|
|