TECHNET Archives

April 2007

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, "Kane, Joseph E (US SSA)" <[log in to unmask]>
Date:
Fri, 20 Apr 2007 13:13:01 -0500
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, David Tremmel <[log in to unmask]>
Subject:
From:
David Tremmel <[log in to unmask]>
Content-Transfer-Encoding:
7bit
In-Reply-To:
Content-Type:
text/plain; charset="us-ascii"
MIME-Version:
1.0
Parts/Attachments:
text/plain (93 lines)
Hello,


I have a copy of the 'Head-in-pillow' document by Alpha Metals.  Is there
any way I could send Steve a copy and he could post it on his site?


Thank you,

David


-----Mensaje original-----
De: TechNet [mailto:[log in to unmask]] En nombre de Kane, Joseph E (US SSA)
Enviado el: Friday, April 20, 2007 1:07 PM
Para: [log in to unmask]
Asunto: [TN] BGA Head In Pillow

Steve was good enough to post some pictures of one of our recent
failures:

http://stevezeva.homestead.com/files/solder_ball_fracture_site_115x.jpg
http://stevezeva.homestead.com/files/solder_ball_SEM_photos_4-13-07_003.
jpg

These are pictures of the underside of the same failed BGA connection,
and
I believe this illustrates a phenomenon discussed here a while back,
called
variously "foot in mud" or "head in pillow" or "ball in socket".
Looking back 
through the archives I couldn't figure out why sometimes the divot
appears on 
the underside of the ball, and sometimes the depression is in the solder

remaining on the land.

I take it that sometimes the BGA ball doesn't melt as fast as the solder
paste, and 
the intact ball may be pulled upward out of the paste when the BGA
warps.  When 
things begin to cool, the ball descends into the pasty solder on the
pad, resulting 
in the "ball in socket".

But if everything does melt together, and the corner warps upward, most
of the 
solder can be pulled up and away by surface tension, leaving a smaller
solder
deposit on the pad.  When things begin to cool, this smaller mass
freezes first, 
and the pasty mass attached to the underside of the BGA settles onto
this hard 
mound, creating "head in pillow".  Like in this case.

Is this fair?

I also saw a number of citations of this link:

http://alphametals.com/products/solder_solutions/pdf/pillowhead.pdf

..which might have led to some good information, but the link appears 
to be broken.  Anyone have a copy of this file, or know a valid
shortcut?

Joe Kane
BAE Systems
Johnson City, NY

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2