Hi Kris,
You have a real problem--it means the plating process used is inadequate for
the PWB design (via diameter, PWB thickness, aspect ratio) and that the
problem is systemic. Not only do you have holes with incomplete Cu coverage,
but the copper that did get plated is very likely of inferior quality in
terms of strength and ductility. The consequence is that you will get barrel
fractures due to the thermal expansion mismatch at soldering process steps.
In my opinion any test/sort/screening effort is a waste of time and
resources; I hope you do not have too many of these PWBs, because they should
be scrapped.
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|