TECHNET Archives

April 1997

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Received:
by ipc.org (Smail3.1.28.1 #2) id m0wJq3x-000BmvC; Tue, 22 Apr 97 19:37 CDT by ipc.org (Smail3.1.28.1 #2) id m0wJpim-000Bq1C; Tue, 22 Apr 97 19:15 CDT
Old-Return-Path:
Date:
Fri, 18 Apr 97 12:43:25 EST
Precedence:
list
Resent-From:
Resent-Sender:
TechNet-d-request TechNet-request [log in to unmask]
X-Status:
Status:
O
X-Mailing-List:
<[log in to unmask]> archive/latest/12148
TO:
Return-Path:
<TechNet-d-request>
From [log in to unmask] Mon Apr 28 17:
09:22 1997
Resent-Message-ID:
<"CfY3o.0.z-F.bILNp"@ipc>
Subject:
From:
X-Loop:
Message-Id:
Parts/Attachments:
text/plain (38 lines)
     
     How does one determine when (if) a sodium permanganate bath is spent??
     
     Problem: Our previously calibrated [Mil-class] etchback cycles for 
     various epoxies are now requiring 2-3 cycles; sections show too much 
     variability from .0005"-.0013"; lots of "gouging" into glass-rich 
     regions with lowest etchback at the copper interface.
     
     Conditions are as follows:
     - All chemistries (solvent swell, permanganate, glass etch) are within 
       vendor specs.
     - NaOH normality: 1.2-1.3
     - NaMnO4 concentration: 60-70 g/l 
     - MnO3 conc. 9 -12 g/l
     - S.G.: 1.13
     - 180 gal tank with 500A continuous electrolytic regeneration
     - swell temp: 175 degF,  permanganate temp: 185 degF
     
     Vendor's tech service won't touch this one - if you want to do 
     chemical etchback "you're on your own"...
     
     Any ideas out there before I dump this bath?
     
     Thanks, Joe Felts 
     PC World, Toronto

***************************************************************************
* TechNet mail list is provided as a service by IPC using SmartList v3.05 *
***************************************************************************
* To subscribe/unsubscribe send a message <to: [log in to unmask]>   *
* with <subject: subscribe/unsubscribe> and no text in the body.          *
***************************************************************************
* If you are having a problem with the IPC TechNet forum please contact   *
* Dmitriy Sklyar at 847-509-9700 ext. 311 or email at [log in to unmask]      *
***************************************************************************



ATOM RSS1 RSS2