Bruce,
Hot bar soldering can be very effective on fine pitch SMT. The two down sides I'm aware of are (1) not a
mass reflow process, (2) potential for creep rupture failure due to the leads being forced down on the pads
while the solder reflows and solidifies. Hughes put out a comprehensive guide to hot bar soldering related
to their hot bar equipment, you might consider contacting them.
Regards,
Ed Hare
--
SEM Lab, Inc.
Scanning Electron Microscopy and Failure Analysis
Snohomish, WA
(425)335-4400
http://www.sem-lab.com
Bruce Robertson wrote:
> Hello everyone,
>
> Who out there knows anything about hot bar soldering?? We are
> considering using an LCD with a TAB driver that requires hot bar
> soldering to the PCB. The problem is I have no experience with this
> process - can anyone please explain to me what is involved, and what
> the pros and cons of using such a process are?
>
> Thanks very much.
>
> Regards,
>
> Bruce Robertson
> Production Engineering
> Mobile Radio Division
> Tait Electronics Ltd.
> ------------------------------------------------------
> 558 Wairakei Road, PO Box 1645
> Christchurch, New Zealand.
> Direct Phone: (64)(3) 3580376 Fax: (64)(3) 358 3603
> Email: [log in to unmask] Internet: http://www.tait.co.nz
> ------------------------------------------------------
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
> To subscribe: SUBSCRIBE TechNet <your full name>
> To unsubscribe: SIGNOFF TechNet
> ################################################################
> Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
> For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
> ################################################################
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|