Hi Neil,
Are you sure you have de-wetting? You may never have had any wetting in the
first place or you may have too much brittle and weak Au-Sn and/or Ag-Sn
intermetallic compounds (IMCs) near the interface, which with upwards of 2
microns of Ag or Au, and particularly with 2 microns each of Ag AND Au, is
likely. You can tell the difference by analyzing the lead surface. If there is
little or no Sn present, you never had wetting, if you have Sn and Ag/Au
present it is the IMCs.
The Ag does not reduce solderability, it is similar to Au in this respect.
With this much Au/Ag underplating with nickel will NOT help. The Ni-underplate
only helps if the brass is not solderable by itself.
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 904-437-8747, Fax: 904-437-8737
E-mail: [log in to unmask]
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|