TECHNET Archives

August 2004

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>, Guenter Grossmann <[log in to unmask]>
Date:
Thu, 26 Aug 2004 10:37:22 +0200
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Edward Szpruch <[log in to unmask]>
Subject:
MIME-Version:
1.0
Content-Transfer-Encoding:
quoted-printable
Content-Type:
text/plain; charset="windows-1255"
From:
Edward Szpruch <[log in to unmask]>
Parts/Attachments:
text/plain (72 lines)
Guenter,
12 microns of copper dissolved by solder ???
I just took a look into IPC 6012A electroplated copper thickness in holes :
minimum thickness allowed in through holes 18-20 microns . In low aspect
ratio blind vias 10-12 microns allowed. So maybe SMD device will be still
attached to the surface, but what about holes ???
There is something wrong.
Edward

Edward Szpruch
Eltek Ltd
P.O.Box 159 ; 49101 Petah Tikva Israel
Tel  ++972 3 9395050 , Fax  ++972 3 9309581
e-mail   [log in to unmask]

> -----Original Message-----
> From: Guenter Grossmann [SMTP:[log in to unmask]]
> Sent: Thu August 26 2004 9:14
> To:   [log in to unmask]
> Subject:      [TN] Antw: [TN] LF Solder Pot
> 
> Victor
> 
> Lead free solder in a wave solder machine does solve a lot of copper from
> a PCB. Trials that where done at ERSA with a solder pot temperature of
> 275°C and a conveyor speed of 1m/min showed that approx. 12um of copper
> have been eaten away from a SMD pad. The only way to avoid this is to
> lower the temperature as far as possible. The lowest wave temperature we
> where able to solder through hole on a 4 layer FR4 with 2 fully metallised
> inner layers was 245°C; 1m/min with SnAgCu. However, this is was the
> lowest limit. We settled now on 250- 255°C for a pilot production.
> 
> Best regards
> 
> Guenter
> 
> EMPA
> Swiss Federal Laboratories  for Materials Testing and Research
> Centre for Reliability
> Guenter Grossmann,  Senior Engineer
> 
> 8600 Duebendorf
> Switzerland
> 
> Phone: xx41 1 823 4279
> Fax :     xx41 1 823 4054
> mail:     [log in to unmask]
> 
> ---------------------------------------------------
> Technet Mail List provided as a service by IPC using LISTSERV 1.8e
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt or (re-start) delivery of Technet send e-mail to
> [log in to unmask]: SET Technet NOMAIL or (MAIL)
> To receive ONE mailing per day of all the posts: send e-mail to
> [log in to unmask]: SET Technet Digest
> Search the archives of previous posts at: http://listserv.ipc.org/archives
> Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
> for additional information, or contact Keach Sasamori at [log in to unmask] or
> 847-509-9700 ext.5315
> -----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2