Morning All,
I've just had a problem that I've seen before, but when I seen this in the
past it was with Tin/Lead soldering, this time it's with Lead Free SAC
soldering.
We're building a board for a customer and one of the caps called out is TDK
PN# CGA3E2X7R1H472K080AD. It's a cap made for conductive epoxy and has
AgPdCu terminations. Well I missed it in the BOM and we've already built
the boards. It was brought to my attention that our rework operator was
having trouble getting the caps to solder and wanted me to take a look at
them. As soon as I seen them I went; "Oh crap..." and then pulled up the
datasheet to verify my suspicions. Here's a photo of the cap:
http://stevezeva.homestead.com/TDK_AgPdCu.jpg
So I made the call that the caps needed to be replaced, with a more
suitable cap like this AVX PN# 06035C472KAT2A. It has a Tin-Nickel
termination and has a X7R dielectric, and is also 4700pf +/- 10%. Some of
the existing caps have solder wet to them, but the solder joints are very
minimal. Knowing how bad these leach I'm leery about leaving them on the
board. Should they be left on the board if they have a minimal solder
joint? The ones that have not wet cannot be touched-up, as soon as you hit
them with a soldering iron the termination dissapears.
Right now we're waiting on the customer to approve the AVX cap.
Steve
--
This email and any attachments are only for use by the intended
recipient(s) and may contain legally privileged, confidential, proprietary
or otherwise private information. Any unauthorized use, reproduction,
dissemination, distribution or other disclosure of the contents of this
e-mail or its attachments is strictly prohibited. If you have received this
email in error, please notify the sender immediately and delete the
original.
______________________________________________________________________
This email has been scanned by the Symantec Email Security.cloud service.
For more information please contact helpdesk at x2960 or [log in to unmask]
______________________________________________________________________
|
|
|