Merely obtaining the calculated percentage of gold by weight in the
solder joint is NOT objective evidence. Where is your limit documented?
There are many other variables besides the percentage by weight.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Sauer, Steve
(Xetron)
Sent: Wednesday, January 31, 2007 2:54 PM
To: [log in to unmask]
Subject: Re: [TN] Maximum Au lead plating thickness
Steve,
I know, long time no hear, too busy keeping the bears off my arse!
The standard states that "the gold shall be removed from 95% of all
surfaces of surface mount components to be soldered regardless of
thickness."
BUT in the same paragraph (3.9.3 of rev D) the following is stated
"These requirements may be eliminated if there is documented objective
evidence available for review that there are no gold related solder
embrittlement problems associated with the soldering process being
used."
So, the objective evidence would be the calculated percentage of gold in
the solder connection.
A sticky situation to be agreed upon with the customer.
Steve
Steve Sauer, CEPM
Sr. Manufacturing Engineer
Northrop Grumman Xetron
Cincinnati, OH
513-881-3368
[log in to unmask]
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Steve Gregory
Sent: Wednesday, January 31, 2007 3:34 PM
To: [log in to unmask]
Subject: Re: [TN] Maximum Au lead plating thickness
Doesn't J-STD-001 say that you can't solder to SMT components with gold
plating no matter what the thickness, and to PTH components unless the
plating is less than 2.5 micro-meters without removing the gold?
-Steve Gregory-
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Louis, Edwin @ CSE
Sent: Wednesday, January 31, 2007 2:26 PM
To: [log in to unmask]
Subject: Re: [TN] Maximum Au lead plating thickness
Ron Bulwith at Alpha Metals(Cookson in Jersey City) researched this and
found that allowable Gold thickness you can solder to with a Tin solder
is ~15-20 micro-inches.You can solder to Gold up to ~200 micro-inches
thick with Lead-Indium solder.
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Bev Christian
Sent: Wednesday, January 31, 2007 2:32 PM
To: [log in to unmask]
Subject: Re: [TN] Maximum Au lead plating thickness
Karen,
You won't find it because it does not exist. You want less than 4% by
weight in the final joint for sure. Dr. Cotts of SUNY Binghampton would
argue for much less.
The reason you won't find a lead plating limit is that the results will
depend on:
1) lead size
2) pad size
3) stencil thickness
These will all affect the final joint concentration.
Bev
RIM
-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Karen Walters Ebner
Sent: Wednesday, January 31, 2007 2:01 PM
To: [log in to unmask]
Subject: [TN] Maximum Au lead plating thickness
Hi
We are looking for the IPC spec that calls out the maximum Au plating
thickness on leads in order to prevent Au embrittlement.
Can anyone provide this to me.
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e To
unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet To temporarily halt or
(re-start) delivery of Technet send e-mail to [log in to unmask]: SET
Technet NOMAIL or (MAIL) To receive ONE mailing per day of all the
posts: send e-mail to [log in to unmask]: SET Technet Digest Search the
archives of previous posts at: http://listserv.ipc.org/archives Please
visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for
additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|