You have a problem with outgassing volatiles. The gas movement in the voids
keeps the solder moving until solidus, which causes poor grain structure
that weakens the joint. The poor grain structure is less reflective adn
therefore shows as grey and not shiny.
What area are you trying to solder? Why is the temperature so far above the
liquidous? (This will make the outgassing problem worse). Reduce the
temperature in stages as much as you can, and monitor the effect at each
stage to determine the best temperature versus soak time. Alternatively,
can you pull a vacuum on the soldering process while the solder is above
liquidous? This would help the outgassing of volatiles.
Pete Duncan
Jonathan A Noquil
<Jonathan.A.Noquil@FAIRCHIL To: [log in to unmask]
DSEMI.COM> cc: (bcc: DUNCAN Peter/Asst Prin Engr/ST Aero/ST Group)
Sent by: TechNet Subject: [TN] Solder Voiding
<[log in to unmask]>
05/11/01 05:55 PM
Please respond to "TechNet
E-Mail Forum."; Please
respond to
Jonathan.A.Noquil
Hello Everyone,
Please help,
Can Anybody explain why too much voiding
occurs when two metal is joined (Top Metal
and Bottom metal)? Eventhough the peak temp is
40 C over than the liquidus temp of the solder.
When a solder is reflowed without top metal
the solder wetting is very good and the appearance
is shiny. But when you put a top metal to be joine
and then X-ray, there are a lot of voids.
I tried to removed the top metal, and the picture
below showed a lot of voids. Another thing is the
color is not shiny but grayish.
(Embedded image moved to file: pic29915.pcx)
The paste is 85Pb/10Sb/5Sn
Peak temp is 290 C
Oven: Conduction
Time until the unit is out: 180 Seconds.
Many thanks to everybody.
Sincerely
Jonathan
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET
Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases >
E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
---------------------------------------------------------------------------------
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------
|
|
|