TECHNET Archives

December 1998

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
Todd Ness <[log in to unmask]>
Date:
Mon, 14 Dec 1998 15:47:25 -0800
Reply-To:
Subject:
From:
Rick Thompson <[log in to unmask]>
Content-Transfer-Encoding:
7bit
In-Reply-To:
Content-Type:
text/plain; charset="Windows-1252"
MIME-Version:
1.0
Parts/Attachments:
text/plain (73 lines)
Todd,

I can't offer a solution, but can validate what you're seeing. We use a
similar TI 100-pin QFP and consistently get bad solder joints. We also
switched from OA 596 to 598 but haven't seen much improvement. There are
some good documents detailing TI's palladium plating including test results
from their testing on the TI web site.  Bottom line is that after talking
with a TI engineer and looking at the documentation noted above, it appears
that paste chemistry is a big factor in soldering to palladium plated leads.
As a result, we're currently evaluating other pastes to see what seems to
work better.

Rick Thompson

> -----Original Message-----
> From: TechNet [mailto:[log in to unmask]]On Behalf Of Todd Ness
> Sent: Monday, December 14, 1998 8:42 AM
> To: [log in to unmask]
> Subject: [TN] Fine-Pitch Soldering Problem
>
>
> Technetters,
>
> We are currently having soldering problems with a QFP 100 package
> part. The part is a TI microprocessor component with a 0.0196" pitch.
> The problem we are having with this part is we are getting
> intermittent opens with corner leads. Other fine-pitch components on
> this board solder fine. We have been building these boards for about 1
> 1/2  years in production with no problems until the last three months.
> I found out that TI recently switched the lead plating for this part
> from Tin/Lead to Nickel/Palladium. The solder paste we were using was
> Kester OA 596. However, due to the inability of this paste to solder
> to palladium parts, we switched to Kester OA 598. The profile was also
> tweeked per Kester's recommendations for soldering to palladium leads.
> All leads for this component and all other components on the board are
> soldering fine with the new paste and new profile, except for some
> intermittent opens on corner leads of the TI part with
> Nickel/Palladium leads. Component leads for this part were inspected
> prior to pick and place for coplanarity. Does anyone have any ideas of
> what may be happening and any recommendations for eliminating this
> problem.
>
> Happy Holidays
>
> ################################################################
> TechNet E-Mail Forum provided as a free service by IPC using
> LISTSERV 1.8c
> ################################################################
> To subscribe/unsubscribe, send a message to [log in to unmask]
> with following text in the body:
> To subscribe:   SUBSCRIBE TechNet <your full name>
> To unsubscribe:   SIGNOFF TechNet
> ################################################################
> Please visit IPC's web site (http://www.ipc.org) "On-Line
> Services" section for additional information.
> For technical support contact Hugo Scaramuzza at
> [log in to unmask] or 847-509-9700 ext.312
> ################################################################
>
>

################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe:   SUBSCRIBE TechNet <your full name>
To unsubscribe:   SIGNOFF TechNet 
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################


ATOM RSS1 RSS2