Hi Jorge and all,
CLCCs have a large CTE mismatch with resin-based PCBs which translate to
large expansion mismatches for larger-sized CLCCs and larger delta-T's. This does
not create higher stresses in solder joints--those are limited by the yield
strength of solder--but larger displacement strains in the SJs and thus larger
plastic deformation. On a cyclic basis, these larger strains lead to much
earlier creep-fatigue failure.
Having thicker solder joints [balls, columns] or compliant leads [QFPs]
reduces the strains in the solder for a given displacement.
PLCCs are quite different, because they lack the large CTE-mismatch with
PCBs.
If you need more information, get a copy of IPC-D-279 and/or IPC-SM-785--or
you could take one of my workshops.
If CLCCs are indeed coming back, people simply have forgotten history, will
be condemned to repeat it, and my consulting business will increase.
Regards,
Werner Engelmaier
Engelmaier Associates, L.C.
Electronic Packaging, Interconnection and Reliability Consulting
7 Jasmine Run
Ormond Beach, FL 32174 USA
Phone: 386-437-8747, Fax: 386-437-8737, Cell: 386-316-5904
E-mail: [log in to unmask], Website: www.engelmaier.com
---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------
|
|
|