TECHNET Archives

September 2011

TechNet@IPC.ORG

Options: Use Monospaced Font
Show HTML Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Sender:
X-To:
TechNet E-Mail Forum <[log in to unmask]>
Date:
Tue, 6 Sep 2011 08:10:25 -0400
Reply-To:
TechNet E-Mail Forum <[log in to unmask]>, Steven Creswick <[log in to unmask]>
Message-ID:
Subject:
From:
Steven Creswick <[log in to unmask]>
Content-Transfer-Encoding:
quoted-printable
In-Reply-To:
Content-Type:
text/plain; charset="iso-8859-1"
MIME-Version:
1.0
Parts/Attachments:
text/plain (220 lines)
Luigi,

Yesterday was a Holiday for most here in the US.  Today, you may get
responses from a more diverse collection of individuals.

In any event, your spec should not be that hard to meet.  If they can not
meet that spec, I would not want their parts.

Steve C

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of
[log in to unmask]
Sent: Tuesday, September 06, 2011 1:58 AM
To: [log in to unmask]
Subject: Re: [TN] Fw: Electroless Ni plating thickness

Thanks for your comments.
It seems it's a very bad idea to accept such Ni plating thickness

CANTAGALLO Luigi




Steven Creswick <[log in to unmask]> 
Envoyé par : TechNet <[log in to unmask]>
05/09/2011 14:47
Veuillez répondre ŕ
TechNet E-Mail Forum <[log in to unmask]>; Veuillez répondre ŕ
Steven Creswick <[log in to unmask]>


A
<[log in to unmask]>
cc

Objet
Re: [TN] Fw: Electroless Ni plating thickness






Cantagallo,

Additional thoughts.  If you are using direct bond copper [DBC] - 

1 - The underlying Cu should be readily solderable.  See what the solder
joint reliability guys say.
2 - The underlying Cu could still diffuse through the thin Ni
3 - Could still have thin Au as well


Steve Creswick
Sr Associate - Balanced Enterprise Solutions
http://www.linkedin.com/in/stevencreswick
              616 834 1883




-----Original Message-----
From: Steven Creswick [mailto:[log in to unmask]] 
Sent: Monday, September 05, 2011 8:07 AM
To: 'TechNet E-Mail Forum'
Subject: RE: [TN] Fw: Electroless Ni plating thickness

Cantagallo,

Hope this helps.

A nominal thickness of 4µm provides enough thickness to prevent leaching, 
in
most cases.  The ±2µm provides the plating operation with a readily
achievable process window, thereby keeping your/their costs down.  Even at 
2
µm one should have good leach resistance and durability.

Three possible issues come to mind.

1 - Even though the rate of dissolution of Ni in the solder is quite slow
[function of temp and alloy], at 0.5µm of Ni you may run into Ni leaching
issues.  Some thick film Cu pastes are fritted, meaning that they bind to
the Al2O3 substrate by mechanical [glass] means.  Some of these pastes
can/do have an excess of frit [glass] at the surface, which makes them
difficult to solder to.  Plating over this surface provides a uniform
surface to solder to.  If your plated surface is in poor condition and you
expose the underlying Cu, the solderability of the Cu may not be all that
good.  There are a lot of "it depends" - on the exact Cu used, Cu firing
conditions, plating control, solder alloy, and solder reflow conditions.

2 - At 0.5µm, the Ni layer may not totally/uniformly cover the underlying
Cu.  If the substrate is subjected to elevated temperatures, the Cu may
diffuse through the thin Ni layer and into the Au layer.  If the substrate
is then allowed to 'sit around' in this condition for prolonged periods of
time, the exposed Cu may oxidize and render the surface only partially
solderable.

3 - Even though you did not ask, if the Ni layer is thin [by accident?], 
it
is possible that the Au layer is also very thin [plating process not in
control] - making item 2 even worse. This can also result in oxidized Ni,
which is also hard to solder to.


If you are thinking about reduced Ni thickness as a cost savings - I would
not do it.  The Ni plating is cheap.  Likely cost you more as a 'special
process'.

If you are asking about reduced Ni thickness because a shipment came in 
that
way - I would send it back and request they ship what you asked for.

Best wishes,

Steve Creswick
Sr Associate - Balanced Enterprise Solutions
http://www.linkedin.com/in/stevencreswick
                616 834 1883





-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of
[log in to unmask]
Sent: Monday, September 05, 2011 5:52 AM
To: [log in to unmask]
Subject: [TN] Fw: Electroless Ni plating thickness

Hello Technetters.

We use a ceramic substrate covered with Cu layer. This Cu layer is plated 
with ENIG process. 
We solder SMD's on it with SnPb process (vapor phase and iron).
The ASTM specifications give a thickness of Ni 4 ± 2 µm.
Where comes from this value ?
What could be an issue with thinner Ni layer like 0.5 µm ?
Thanks to answer.

Best regards,

CANTAGALLO Luigi

______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------



______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to 
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to 
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 
847-615-7100 ext.2815
-----------------------------------------------------


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------


______________________________________________________________________
This email has been scanned by the MessageLabs Email Security System.
For more information please contact helpdesk at x2960 or [log in to unmask] 
______________________________________________________________________

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 16.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
For additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2