Hi Julien! Now that's a question I would have never anticipated being asked
- you want to oxidize a component finish! The real trick is to create an
oxidized surface that is realistic so that your operator's are not trying
to solder the impossible. But you are in luck - the JSTD-002A committee
asked the question a year ago but in terms of "is steam conditioning the
most appropriate conditioning environment to use". And since I didn't have
a Master Thesis topic at the time I chose to research the oxidation of tin.
My thesis is nearly complete (words of wisdom - get your advanced degree
when you aren't working and have a family!) and I will be reporting the
results in 2002. My recommendation is an 8 hour bake at 125C - the
oxidation thickness and composition is similar to the oxidation condition
after 1 year of ambient storage. Good luck.
Dave Hillman
Rockwell Collins
[log in to unmask]
Julien Bouchard <[log in to unmask]>@ipc.org> on 11/05/2001
12:20:05 PM
Please respond to "TechNet E-Mail Forum." <[log in to unmask]>
Sent by: TechNet <[log in to unmask]>
To: [log in to unmask]
cc:
Subject: [TN] Looking for a way to oxidized tin-lead plated component
Hi,
We implement a more structured training program and in a part of
this
programs, we want to train the operator by give them pratice on oxidized
tin-lead plated component. Does someone know a way to accelerate the
natural
oxiditation process of tin-lead alloys using in electronic to simulate and
heavily oxidized component ? Thank.
Julien Bouchard ing. stag.
Matrox - Process Engineer
---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------