TECHNET Archives

March 2003

TechNet@IPC.ORG

Options: Use Monospaced Font
Show Text Part by Default
Condense Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Content-Type:
text/plain; charset="iso-8859-1"
Sender:
Subject:
From:
"Barmuta, Mike" <[log in to unmask]>
Date:
Tue, 18 Mar 2003 10:02:31 -0800
MIME-Version:
1.0
X-To:
Sencer Sofuoglu <[log in to unmask]>, "TechNet E-Mail Forum." <[log in to unmask]>
Reply-To:
"TechNet E-Mail Forum." <[log in to unmask]>, "Barmuta, Mike" <[log in to unmask]>
Parts/Attachments:
text/plain (142 lines)
Sofu: When acid Cu plating baths stay idle for long periods of time the
certain components of the brightener systems can selectively decompose. This
may not be picked up by CVS. I guessing this may be what you saw. Dummy
plating the bath and readjusting the brighteners should bring it back in
good condition.
You still may want to do some type of carbon treat occasionally to strip out
all the brightener and start fresh.


Regards

Mike Barmuta

-----Original Message-----
From: Sencer Sofuoglu [mailto:[log in to unmask]]
Sent: Tuesday, March 18, 2003 8:33 AM
To: 'Barmuta, Mike'; 'TechNet E-Mail Forum.'
Subject: RE: [TN] Iron for Electrolytic Copper Plating


Mike,

Thanks for the help.

Actually it is a one panel test bath that I made up 2 years ago. I
introduced only a few panels with dry film to the bath. I did not carbon
treat but I don't think organic contamination is the case. Sometimes bath
stay idle for long time and then I need to do long time dummy plating before
start testing again. It has been running good since last dummy plating.

Control of additives are done by CVS to measure brightener and leveller
separately. When I asked about iron concentration, readings was good with
brightener and leveller. The CVS and Hull Cell did not show anything
unusual. Later, I started to read high brightener and low leveller
concentration. Now readings are normal after dummy plating and problem seems
to be solved.

I didn't understand why brightener concentration increased and CVS did not
show anything. I know that CVS is a very sensitive device and readings can
be erroneous. But we run same procedure of CVS for also production bath and
readings are stable.

Best regards,

Sofu




-----Original Message-----
From: Barmuta, Mike [mailto:[log in to unmask]]
Sent: Monday, March 17, 2003 4:14 PM
To: 'TechNet E-Mail Forum.'; 'Sencer Sofuoglu'
Cc: Barmuta, Mike
Subject: RE: [TN] Iron for Electrolytic Copper Plating


Sofu: Iron contamination at 70ppm will not cause LCD dullness. It will
create dull LCD deposits in the 800-1000ppm range and above.

If the main constituents are in balance, I would suspect organic
contamination, anode polarization or insufficient brightener.

A couple of things to consider:
1.How do you verify the brightener is at the proper concentration? Most
brightener systems are multi-component and must be kept in balance. Are you
using CVS, Hull cells, chromatography? Obviously low brightener will cause
dullness. You can usually 2X the brightener concentration without affecting
the deposit.

2.Take a look at your anodes, the film should have a black uniform velvety
appearance. The anode bags should be clean and free of any build up on the
bottom. Make sure the anode material is of sufficient size and not de-plated
done to nothing. You don't want anode nuggets plated down to the size of pea
gravel or slab anodes that look like spears or dog bones.

3. Check your chloride PPM, low chloride as well as high chloride will cause
dullness. The high chloride will also show up as a white-gray film on your
anodes.

4. Are you properly(off line)batch carbon treating the bath and not just
running it thru some carbon packs in your filter chamber?

There are many things that will cause LCD dullness those mentioned above are
some of the most common.


Regards

Michael Barmuta

Staff Engineer

Fluke Corp.

Everett WA

425-446-6076

-----Original Message-----
From: Sencer Sofuoglu [mailto:[log in to unmask]]
Sent: Friday, March 14, 2003 12:39 PM
To: [log in to unmask]
Subject: [TN] Iron for Electrolytic Copper Plating


Hello,

We see some dullness at low current density area and I consider that one of
the reasons can be iron concentration. Current concentration is 70ppm. What
kind of Iron concentrations do you control your bath? What would be the
result of high or low iron concentrations? Any comment appreciated.

Regards,

Sofu

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/html/forum.htm for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2