TECHNET Archives

January 2001

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
Nancy Trumbull <[log in to unmask]>
Reply To:
TechNet E-Mail Forum.
Date:
Mon, 29 Jan 2001 12:11:25 -0500
Content-Type:
text/plain
Parts/Attachments:
text/plain (103 lines)
Gaby,
Here is hoping your day is going well.  I'm not sure of your question. I believe you are asking why the illustration show one thing and the written criteria shows another.  If so look on page 1-2 of IPC610C and in section 1.2 it states
" In the case of a discrepancy, the description or written criteria always takes precedence over the illustration. " 
Or are you wanting to understand what the 6.5.2. is saying.
Hope this helps.
Nancy T.

>>> [log in to unmask] 01/29/01 10:06AM >>>
Par.6.5.2. of IPC-A-610C:
Acceptable-Class 1,2,3
-Exposed copper on vertical conductor edges
-Exposed basis metal at ends of component leads
But... The picture shows exposed copper alloy of lead base matrial.
What's the catch???
Gaby

> ----------
> From:         Rick Howieson[SMTP:[log in to unmask]] 
> Reply To:     TechNet E-Mail Forum.;Rick Howieson
> Sent:         ???? ??? 29 ????? 2001? 16:33
> To:   [log in to unmask] 
> Subject:      Re: [TN] fractured joints
> 
> Careful Doug...nowhere does the spec indicate trimmed leads must be
> covered
> with solder. An example, how would YOU explain the acceptability of an
> exposed vertical trace on a board that has been SnPb plated and fused?
> Rick
> 
> -----Original Message-----
> From: Douglas Pauls [mailto:[log in to unmask]] 
> Sent: Monday, January 29, 2001 7:01 AM
> To: [log in to unmask] 
> Subject: Re: [TN] fractured joints
> 
> 
> The IPC standard states that all clipped leads must either be  reflowed or
> checked under 10X magnification. Is this just a standard for single  sided
> boards? If you have a double sided board and a good fillet on the
> component side of the board and you clipped the leads on the solder side
> what  would be the cause of concern if a joint is fractured on the solder
> side?
> 
> *One of the reasons that the specifications want you to check the clipped
> leads, or better yet, reflow the solder to cover the clipped lead is so
> that you cover the exposed metal of the lead which may corrode.  I have
> seen many cases where a ferrous core of the lead is exposed by the
> clipping
> process, which then corrodes in service.  If that exposed metal was
> covered
> with tin-lead, that corrosion does not occur.
> 
> Not quite what you were looking for, but something to think about.
> 
> Doug Pauls
> Rockwell Collins
> 
> 
> --------------------------------------------------------------------------
> --
> -----
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message: SET
> Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources & Databases >
> E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
> --------------------------------------------------------------------------
> --
> -----
> 
> --------------------------------------------------------------------------
> -------
> Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
> To unsubscribe, send a message to [log in to unmask] with following text in
> the BODY (NOT the subject field): SIGNOFF Technet
> To temporarily halt delivery of Technet send the following message: SET
> Technet NOMAIL
> Search previous postings at: www.ipc.org > On-Line Resources & Databases >
> E-mail Archives
> Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
> additional
> information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
> ext.5315
> --------------------------------------------------------------------------
> -------
> 

---------------------------------------------------------------------------------
Technet Mail List provided as a free service by IPC using LISTSERV 1.8d
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt delivery of Technet send the following message: SET Technet NOMAIL
Search previous postings at: www.ipc.org > On-Line Resources & Databases > E-mail Archives
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
---------------------------------------------------------------------------------

ATOM RSS1 RSS2