At 04:13 PM 7/31/00 -0500, you wrote:
>Hello TechNet:
>We performed some experiments on Immersion White Tin boards and found the
>following . . . . First, we had no problems with solder paste application.
>Second, no problems with vision systems, etc., and part placement. Third,
>solder joints looked pretty good . . i.e. . no problems. Here is the
>kicker. The mounting holes on the top side were white tin. The mounting
>holes need to be very flat for good contact so we do not apply solder paste
>to these holes. The white tin, after exposure to humidity of the
>environmental chambers looked very oxidized and a flaky white powdery like
>substance was observed. Also under some RF type connectors, the white
>powdery like substance was observed. The powdery like flaky substance did
>not show up under any other components only the gold RF connectors.
>
>What experience have any of you had with the immersion white tin process?
>Any ideas, thoughts, etc., on the powdery white substance??? We are going to
>have our "product assurance forensic lab" analyze it and see what they come
>up with, but we also thought it a good idea to tap the intelligence of the
>TechNet World as well.
>
>Ron Hollandsworth
>ITT
>
>
>************************************
>If this email is not intended for you, or you are not responsible for the
>delivery of this message to the addressee, please note that this message may
>contain ITT Privileged/Proprietary Information. In such a case, you may not
>copy or deliver this message to anyone. You should destroy this message and
>kindly notify the sender by reply email. Information contained in this
>message that does not relate to the business of ITT is neither endorsed by
>nor attributable to ITT.
>************************************
>
>##############################################################
>TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
>##############################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with
>following text in
>the body:
>To subscribe: SUBSCRIBE TECHNET <your full name>
>To unsubscribe: SIGNOFF TECHNET
>##############################################################
>Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
>information.
>If you need assistance - contact Keach Sasamori at [log in to unmask] or
>847-509-9700 ext.5315
>##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Keach Sasamori at [log in to unmask] or
847-509-9700 ext.5315
##############################################################
|