In-Reply-To:
Content-Type:
text/plain; charset="US-ASCII"
MIME-Version:
1.0
Parts/Attachments:
text/plain (144 lines)
Additionally I have seen some silicones and polymers suffer cure
inhibition/poor adhesion on high tin content alloys especially if there are
any tin compounds on the tin. These soft spots and low adhesion areas
look/behave similarly to poor cure overall but are localised.

Regards
 
 
Mike

-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Joyce Koo
Sent: Tuesday, June 09, 2009 1:45 PM
To: [log in to unmask]
Subject: Re: [TN] cracking of coating

Your coating is not cured.  Check instruction of the product about tack time
and full strength develop time.  Contact your coating vendor application
engineer. 
--------------------------
Sent using BlackBerry


----- Original Message -----
From: TechNet <[log in to unmask]>
To: [log in to unmask] <[log in to unmask]>
Sent: Tue Jun 09 07:36:40 2009
Subject: [TN] cracking of coating

Hello Technet,

We have an issue of cracking of silicone conformal coating on tin coated
pcb.
Please read below whole procedure of our process of wave soldering and 
reflow soldering.

Here is our process from beginning of assembly to end of temperature test:

1- SMT components:

Print  lead free No-Clean solder paste on the PCB.

Put SMT components on PCB.

Oven reflow process to solder components.

2- Trough holes components:

Install through holes components.

Solder the through holes components in lead free solder wave.

Liquid flux (No clean) is sprayed on bottom side of the PCB.

            The PCB goes into pre-heating section.

            The bottom side is dipped in SN liquid alloy at 260'C.

            The PCB is cooled down at room temperature.

3- Tests:

            Electrical/functionality tests are done on each unit.

4- Coating:

            Spray with gun (100% silicone not mixed with thinner).

            1st layer is applied on bottom side of the PCB.

            2nd layer is applied on bottom side of the PCB at least 10
minutes 
after the first layer.

            PCB's are left to dry 1 hour.

            1st layer is applied on top side of the PCB.

            2nd layer is applied at least 10 minutes after first layer.

            PCB's are left to dry 1 hour.

            The PCB's are cured 1 hour in oven at 65'C.

            Inspection with UV light.

5- Temperature test.

            PCB's are put in environmental chamber at -30'C.   
            After 1 hour, cracks are visible.

            PCB's are left at -30'C about 15 hours.

            More cracks have appeared.  Air pockets and humidity are present

under the coating.

            Coating can be rubbed off the PCB using small tool or pick.

 

I've included picture of cracked coating and a report of the tests we made.

Thanking you in advance for your help in this matter.

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask] or
847-615-7100 ext.2815
-----------------------------------------------------

---------------------------------------------------------------------
This transmission (including any attachments) may contain confidential
information, privileged material (including material protected by the
solicitor-client or other applicable privileges), or constitute non-public
information. Any use of this information by anyone other than the intended
recipient is prohibited. If you have received this transmission in error,
please immediately reply to the sender and delete this information from your
system. Use, dissemination, distribution, or reproduction of this
transmission by unintended recipients is not authorized and may be unlawful.


***This email, its content, and any files transmitted with it, are intended solely for the addressee(s) and may be legally privileged and/or confidential. If you are not the intended recipient, please contact the sender by return and delete the material from any computer. Any review, retransmission, dissemination, or other use of, or taking of any action in reliance upon this information by persons or entities other than the intended recipient is prohibited.

Messages sent via this medium may be subjected to delays, non-delivery, and unauthorized alteration. This email has been prepared using information believed by the author to be reliable and accurate, but Indium Corporation makes no warranty as to accuracy or completeness. Indium Corporation does not accept responsibility for changes made to this email after is was sent. Any opinions or recommendations expressed herein are solely those of the author. They may be subject to change without notice.***

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 15.0
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-615-7100 ext.2815
-----------------------------------------------------

ATOM RSS1 RSS2