We plate tin-lead over nickel regularly, either immediately or after
another layer of resist. We're running a Watts bath (nickel chloride,
nickel sulfate, boric acid) rather than sulfamate. The activation of the
nickel surface before the tin-lead plating is critical. If the nickel
plate has been dried, there's an initial PC-455 bath to clean the
surface, then the steps are water rinse, 40% hydrochloric etch, rinse,
10% fluoboric etch, rinse, tin-lead plating. Once started from nickel to
tin-lead, the timings are tightly controlled, certainly no long dwells in
the rinses or etches.
Steve Axdal
[log in to unmask]
Tom Bresnan wrote:
> All:
>
> Is there a preferred nickel I should be trying to plate solder on top
> of? We're struggling with plating tin lead on top of nickel and it's
> subsequent reflow after soldermask. Anyone have any suggestions? We're
> seeing dewetting and I'm wondering how many others out there are
> trying to do this. We currently use a nickel sulfamate bath, if that
> has any bearing... I'm not sure of activators and such, but if you
> think it's important, I'll find them.
>
> Thanks in advance all...
>
> Regards
>
> Tom Bresnan
> [log in to unmask]
>
> PS. Please respond direct to me as well as to the forum. I'm presently
> disconnected from the service.
snip--------------------------
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|