Stephen,
Is it possible that the mask is over cured? Maybe somewhat embrittled? The
problem seems like more of an adhesion problem as you suggested. If the mask
in undercured, a thermal bump should give the mask some additional
crosslinking.
If the mask is a two part system, the shop may have had some component
mixing problems or the mask pot life was nearing its end.
Good luck,
Mike Carano
-----Original Message-----
From: Stephen R. Gregory [SMTP:[log in to unmask]]
Sent: Friday, February 11, 2000 8:12 AM
To: [log in to unmask]
Subject: [TN] Solder mask failing tape test..
Mornin' all!!
This morning I got a email from one of our buyers telling me that
one of the
boards at one of our fab shops is being held-up because it doesn't
pass their
solder mask tape test. My buyer said that they told him that the
mask is only
coming off the via's, and it was because of uncured mask. The mask
is a LPI
and the via's aren't meant to be tented. Also the board doesn't go
through
wave solder as the only through-hole is hand soldered because it
goes up
through the board from the bottomside.
My buyer is asking me if we should accept the boards. I have a few
concerns.
One thing is that if there is uncured mask at the via's, what
guarantees are
there that there isn't more at other places on the board? Shouldn't
uncured
mask be a simple thing to fix by either baking the PCB (if it's a
thermal
cure), or exposing it to more UV (if it's a UV cure)?
Further still, does uncured mask come off in a tape test? Or is mask
coming
off from a tape test more an indication of an adhesion problem from
contamination?
Thanks in advance for all replies,
-Steve Gregory-
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV
1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with
following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for
additional
information.
If you need assistance - contact Gayatri Sardeshpande at
[log in to unmask] or
847-509-9700 ext.5365
##############################################################
##############################################################
TechNet Mail List provided as a free service by IPC using LISTSERV 1.8c
##############################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in
the body:
To subscribe: SUBSCRIBE TECHNET <your full name>
To unsubscribe: SIGNOFF TECHNET
##############################################################
Please visit IPC web site (http://www.ipc.org/html/forum.htm) for additional
information.
If you need assistance - contact Gayatri Sardeshpande at [log in to unmask] or
847-509-9700 ext.5365
##############################################################
|
|
|