Hello Tom,
I have plated Sn/Pb over nickel. I have also used a nickel sulfamate bath
operating at around 54C. I did not see dewetting after reflow.
The Sn/Pb plating was done immediately after the nickel plating. Following
the Ni electrodeposition, the surface was rinsed, dipped into a dilute
nitric acid bath, and then rinsed again. The Sn/Pb plating was initiated
before the surface was allowed to dry. I was using a methane sulfonic acid
based bath for the Sn/Pb plating.
Best Regards,
Christine
At 12:38 PM 6/18/98 -0400, you wrote:
> All:
>
> Is there a preferred nickel I should be trying to plate solder on top
> of? We're struggling with plating tin lead on top of nickel and it's
> subsequent reflow after soldermask. Anyone have any suggestions? We're
> seeing dewetting and I'm wondering how many others out there are
> trying to do this. We currently use a nickel sulfamate bath, if that
> has any bearing... I'm not sure of activators and such, but if you
> think it's important, I'll find them.
>
> Thanks in advance all...
>
> Regards
>
> Tom Bresnan
> [log in to unmask]
>
> PS. Please respond direct to me as well as to the forum. I'm presently
> disconnected from the service.
>
********************************************************
Christine Lizzul Rinne
Graduate Student
Dept. Of Materials Science and Engineering
North Carolina State University
Box 7907
Raleigh, NC 27695-7907
(919) 248-1107 TEL
(919) 248-1455 FAX
NCSU
http://vims.ncsu.edu/matsci/
*********************************************************
################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe: SUBSCRIBE TechNet <your full name>
To unsubscribe: SIGNOFF TechNet
################################################################
Please visit IPC web site (http://jefry.ipc.org/forum.htm) for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################
|
|
|