text/plain (181 lines)
And of course this book is available from the SMTA.  SMTA members can buy
it for $64.95 (look! It's $.05 cheaper!), and non-members for $84.95.
Order via http://www.smta.org.

UPS ground shipping is free!

Regards,

-David


At 12:21 PM 10/1/98 -0400, you wrote:
>Don't forget about the wire bonding bible:
>
>Wire Bonding in Microelectronics Materials, Processes, Reliability & Yield
>          George Harman
>          ISBN: 0-07-032619
>          IMAPS Member: $65, Nonmember: $115
>
>http://www.imaps.org/pubs.htm
>
>
>
>
>----------
>From:  Terry Regan [SMTP:[log in to unmask]]
>Sent:  Wednesday, September 30, 1998 3:35 PM
>To:  [log in to unmask]
>Subject:  Re: [TN] Fab:  Multiple surface finishes
>
>Glenn and Michael,
>    It is true that 30u" is typically an acceptable gold thickness for
>thermosonic bonding.  In fact, we have customers that have had tremendous
>success bonding to 17u".  There are many criteria which can affect the
>bondability including the Nickel underlay, the pourosity of the Nickel and
the
>Gold platings, the chuck temperature, the plasma cleaning process, etc.  The
>real catch is understanding and characterizing your bonding equipment with
the
>product supplied by your substrate manufacturer.  Performance of a given
>thickness of gold from one supplier is probably not the same as that
thickness
>from another supplier.  There is a definite need to form a relationship with
>your supplier and work with them to define the optimum parameters.  A DOE
would
>probably do the trick.  (then don't let your buyers go on a "price" hunt for
>suppliers)
>
>Terry Regan
>HADCO
>
>____________________Reply Separator____________________
>Subject:    [TN] Fab:  Multiple surface finishes
>Author: "Alderete; Michael" <[log in to unmask]>
>Date:       9/30/98 2:44 PM
>
>Glenn-
>
>Hadco (Watsonville CA) recently talked us into 30 microinches Au, vs.
>our original 50 microinch callout, on BT laminate. We established that
>reliable Au wire wedge bonds could be made at 30, before we approved the
>order. We're now thinking that we could make good wire bonds to
>something less than 30, but we haven't tried. Maybe Hadco (or someone
>else) can recommend minimum Au plating for Au wire bonding AND
>(eutectic) soldering.
>
>-Michael Alderete
>
>
>You wrote...
>------------------------------
>
>Date:    Wed, 30 Sep 1998 10:31:54 PDT
>From:    glenn pelkey <[log in to unmask]>
>Subject: Fab:  Multiple surface finishes
>
>Hello all,
>
>     I'm looking for information on how to build a board with both soft
>gold and solder as outer layer surface finishes.  We want to make sure
>it is manufacturable before designing it.  The only thing I have now are
>examples with edge connectors.  The gold and solder would be at select
>locations throughout the board.
>
>     In case you're wondering why, I'll tell you.  We want to increase
>the gold thickness to greater than 70 microinches for wire bonding.
>But, this product also has screened solder for SMT.  Since sceening
>limits the amount of solder, gold embrittlement becomes an issue.  I
>calculated 3.7% of gold by weight at 70 microinches.  I know opinions
>vary here, but I think everyone can agree that this is at least a
>concern.
>
>      What do you think?  How hard is this to do?  Contamination,
>increased cost, other reliabilty or quality issues to trade off?
>
>Thanks for all your help.
>
>Glenn Pelkey
>Maxtek Components Corp.
>[log in to unmask]
>[log in to unmask]
>
>______________________________________________________
>Get Your Private, Free Email at http://www.hotmail.com
>
>------------------------------
>
>################################################################
>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with
following text
>in the body:
>To subscribe:   SUBSCRIBE TechNet <your full name>
>To unsubscribe:   SIGNOFF TechNet
>################################################################
>Please visit IPC's web site (http://www.ipc.org) "On-Line Services"
section for
>additional information.
>For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700
>ext.312
>################################################################
>
>################################################################
>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with
following text in the body:
>To subscribe:   SUBSCRIBE TechNet <your full name>
>To unsubscribe:   SIGNOFF TechNet
>################################################################
>Please visit IPC's web site (http://www.ipc.org) "On-Line Services"
section for additional information.
>For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
>################################################################
>
>################################################################
>TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
>################################################################
>To subscribe/unsubscribe, send a message to [log in to unmask] with
following text in the body:
>To subscribe:   SUBSCRIBE TechNet <your full name>
>To unsubscribe:   SIGNOFF TechNet
>################################################################
>Please visit IPC's web site (http://www.ipc.org) "On-Line Services"
section for additional information.
>For technical support contact Hugo Scaramuzza at [log in to unmask] or
847-509-9700 ext.312
>################################################################
>

David Gonnerman
Director of Publications

Plan now to attend:
*Electronics Assembly Expo*
Providence, RI; Oct. 24-29, '98; http://www.ipc.org/html/assemexpo.htm

SURFACE MOUNT TECHNOLOGY ASSOCIATION
             Enabling members to achieve success
        in surface mount and companion technologies
    through education, training and access to knowledge.

5200 Willson Road, Suite 215, Edina, MN  55424-1343
           612-920-7682  F 612-926-1819
               [log in to unmask]   www.smta.org

################################################################
TechNet E-Mail Forum provided as a free service by IPC using LISTSERV 1.8c
################################################################
To subscribe/unsubscribe, send a message to [log in to unmask] with following text in the body:
To subscribe:   SUBSCRIBE TechNet <your full name>
To unsubscribe:   SIGNOFF TechNet 
################################################################
Please visit IPC's web site (http://www.ipc.org) "On-Line Services" section for additional information.
For technical support contact Hugo Scaramuzza at [log in to unmask] or 847-509-9700 ext.312
################################################################


ATOM RSS1 RSS2