TECHNET Archives

December 2003

TechNet@IPC.ORG

Options: Use Proportional Font
Show Text Part by Default
Show All Mail Headers

Message: [<< First] [< Prev] [Next >] [Last >>]
Topic: [<< First] [< Prev] [Next >] [Last >>]
Author: [<< First] [< Prev] [Next >] [Last >>]

Print Reply
Subject:
From:
"Stolar, Paul W" <[log in to unmask]>
Reply To:
TechNet E-Mail Forum.
Date:
Wed, 17 Dec 2003 13:21:15 -0600
Content-Type:
text/plain
Parts/Attachments:
text/plain (249 lines)
It seems to be a film on some leads. 

Paul Stolar
Materials/Reliability Engineer
Manufacturing Reliability Lead Engineer
Baker Atlas
713-625-5376


-----Original Message-----
From: TechNet [mailto:[log in to unmask]] On Behalf Of Bev Christian
Sent: Wednesday, December 17, 2003 11:33 AM
To: [log in to unmask]
Subject: Re: [TN] Blue leads

Paul,
Is the blue color on all leads or just some?  Is it close to the solder
from the solder paste or just on the tops of lead surfaces?  I am
wondering if your joints have been contaminated with copper from the
leads and you are seeing copper salts.
Bev Christian
Research in Motion

-----Original Message-----
From: Dave Hillman [mailto:[log in to unmask]]
Sent: December 16, 2003 12:58 PM
To: [log in to unmask]
Subject: Re: [TN] Blue leads


Hi Vlad! Sorry, I didn't mean to imply that there is free silver on the
surface. The microstructure of a Sn96Ag4 solder joint can be Sn phase
with
in a Sn-Ag3Sn eutectic matrix or it can be Sn phase with lots of Ag3Sn
intermetallic needles. I don't know what the influence the Sn with have
on
the Ag3Sn eutectic in terms of oxidation but I was guessing that
potentially a Ag sulfide might come into play (Ag sulfide has a purplish
appearance). Another guess would be that Paul has a Sn oxide species
that
the Ag is influencing such that it has a darker visual appearance than
typical. Either idea may be way off base too but looking at what Paul
had I
thought I would venture a couple of guesses. Any reason you are leaning
toward XPS analysis instead of Auger analysis?

(That's probably way more metallurgy discussion than some of the Technet
crew was looking for but the SnAg system is much more "interesting" than
the SnPb system).

Dave Hillman
Rockwell Collins



                      "Vladimir
                      Igoshev"                 To:       "TechNet E-Mail
Forum." <[log in to unmask]>, <[log in to unmask]>
                      <[log in to unmask]        cc:
                      >                        Subject:  RE: [TN] Blue
leads

                      12/16/2003 11:00
                      AM






Dave,

Why do you think it may be some silver based "film"? It shouldn't be any
"free" silver in the solder alloy (there is almost nothing in the solid
solution), but only the intermetallics. I think XPS can be run to figure
out what is on the surface.

Regards,

Vladimir Igoshev,
Research in Motion



-----Original Message-----
From: Dave Hillman [mailto:[log in to unmask]]
Sent: Monday, December 15, 2003 5:37 PM
To: [log in to unmask]
Subject: Re: [TN] Blue leads


Hi folks! Well, as Steve mentioned,  the typical "blue" tint seen on a
solder joint is the result of Pb oxide dominating the solder joint
surface
instead of the usual Sn oxide. Overcleaning is a classic way of
producing
"Barney pwbs" but since Paul is using an Sn96Ag4 solder alloy we can't
be
dealing with Pb oxide. I don't know of any Sn oxide species that are
"blue"
in appearance. My guess is that the blue appearance is due to some Ag
surface species - silver sulfide can have a "blueish" appearance. If you
had a flat enough surface you can use the SERA equipment to identify
some
silver surface species (silver oxide, silver chloride, silver sulfide).
I'll see if any of my references can provide any help. A majority of the
time these types of observations have only cosmetic impact and not a
product integrity impact  (someday the bright and shiny myth will be
extinct!).

Dave Hillman
Rockwell Collins
[log in to unmask]




                      Steve Gregory
                      <[log in to unmask]        To:       [log in to unmask]
                      M>                       cc:
                      Sent by: TechNet         Subject:  Re: [TN] Blue
leads
                      <[log in to unmask]>


                      12/15/2003 03:23
                      PM
                      Please respond to
                      "TechNet E-Mail
                      Forum."; Please
                      respond to
                      SteveZeva






Hi Paul!

I had an experience with what we called "Blue Solder" once, but it was
traced
back to our cleaning process...you can see a picture of it on my web
page
at:

http:www.stevezeva.homestead.com and look at "Blue Solder". What we
discovered was that the airknife cycle in between the wash and rinse
cycle
was drying
out the chemistry on the solder joints before we could get it rinsed of.
Once
we shortened the airkife cycle, the appearance went away. This was
dealing
with
63/37 solder too, not SN96 solder...

Dave Hillman has some pictures on my page next to the "Blue Solder" one,
he
called "Barney Boards" because of the purple appearance of the solder. I
can't
quite remember what the situation was with that...maybe he will see this
and
refresh our memories.

-Steve Gregory-


> We just ran a long time heat run at 175C on a board made with
Sn96/4Ag.
> The leads turned blue.
>
> I don't have my CRC handy. What caused the blue? Is it silver halide?
IS
> there another tin oxide I am not aware of which turns blue? Or even
> copper?
>
>
>
>
> Paul Stolar
> Materials/Reliability Engineer
> Manufacturing Reliability Lead Engineer
> Baker Atlas
> 713-625-5376
>

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16
for additional information, or contact Keach Sasamori at [log in to unmask]
or
847-509-9700 ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text
in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to
[log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to
[log in to unmask]: SET Technet Digest
Search the archives of previous posts at:
http://listserv.ipc.org/archives
Please visit IPC web site
http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional
information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700
ext.5315
-----------------------------------------------------

---------------------------------------------------
Technet Mail List provided as a service by IPC using LISTSERV 1.8e
To unsubscribe, send a message to [log in to unmask] with following text in
the BODY (NOT the subject field): SIGNOFF Technet
To temporarily halt or (re-start) delivery of Technet send e-mail to [log in to unmask]: SET Technet NOMAIL or (MAIL)
To receive ONE mailing per day of all the posts: send e-mail to [log in to unmask]: SET Technet Digest
Search the archives of previous posts at: http://listserv.ipc.org/archives
Please visit IPC web site http://www.ipc.org/contentpage.asp?Pageid=4.3.16 for additional information, or contact Keach Sasamori at [log in to unmask] or 847-509-9700 ext.5315
-----------------------------------------------------

ATOM RSS1 RSS2